JP2000132818A - Method of manufacturing magnetoresistive film, magnetoresistive film using the same, and thin-film magnetic head - Google Patents

Method of manufacturing magnetoresistive film, magnetoresistive film using the same, and thin-film magnetic head

Info

Publication number
JP2000132818A
JP2000132818A JP10306557A JP30655798A JP2000132818A JP 2000132818 A JP2000132818 A JP 2000132818A JP 10306557 A JP10306557 A JP 10306557A JP 30655798 A JP30655798 A JP 30655798A JP 2000132818 A JP2000132818 A JP 2000132818A
Authority
JP
Japan
Prior art keywords
film
substrate
layer
magnetic field
permalloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP10306557A
Other languages
Japanese (ja)
Inventor
Masashi Michijima
正司 道嶋
Tomohisa Komoda
智久 薦田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sharp Corp
Original Assignee
Sharp Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sharp Corp filed Critical Sharp Corp
Priority to JP10306557A priority Critical patent/JP2000132818A/en
Publication of JP2000132818A publication Critical patent/JP2000132818A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To obtain high sensitivity and large exchange coupling magnetic field by forming a first ferromagnetic layer, nonmagnetic layer, second ferromagnetic layer and antiferromagnetic layer and applying a high frequency bias on the substrate during the formation of the first ferromagnetic layer. SOLUTION: A target is disposed in a horizontal plane and films are formed on a film forming face of a magnetoresistance effect film tilted by a specified angle from the horizontal plane. A permalloy film is formed by the RF conventional sputtering method, and during the permalloy film formation, a high frequency substrate bias is applied so that deterioration in the soft magnetic characteristics can be prevented even on a plane tilted from the horizontal state. The optimum high frequency substrate bias is properly determined according to the angle of the substrate and to the size of the film forming chamber. The permalloy film thus obtd. is used to produce a magnetoresistance effect film(spin valve film).

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、磁気記録用再生ヘ
ッドあるいは磁気センサ等に使用されるスピンバルブ構
造の磁気抵抗効果膜の製造方法、それを用いた磁気抵抗
効果膜、並びに薄膜磁気ヘッドに関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method of manufacturing a magnetoresistive film having a spin valve structure used for a magnetic recording reproducing head or a magnetic sensor, a magnetoresistive film using the same, and a thin film magnetic head. Things.

【0002】[0002]

【従来の技術】磁気ディスクなどの磁気記録装置におい
ては、記録密度の向上に伴い、磁気ヘッドの高性能化が
求められている。
2. Description of the Related Art In a magnetic recording apparatus such as a magnetic disk, a higher performance of a magnetic head is required with an increase in recording density.

【0003】即ち、記録ヘッドでは媒体の高保磁力化に
伴い、飽和磁束密度の大きな材料が要求されている。
That is, in the recording head, a material having a large saturation magnetic flux density is required as the coercive force of the medium increases.

【0004】また、再生ヘッドでは、媒体の小型化に伴
う相対速度の低下に対して、従来の誘導型ヘッドに変え
て、磁気抵抗効果を利用したいわゆるMRヘッドを用い
ることで再生出力の増加が図られている。
[0004] In the read head, in response to a decrease in the relative speed due to the downsizing of the medium, a so-called MR head utilizing the magnetoresistive effect is used instead of the conventional inductive head, so that the read output increases. It is planned.

【0005】さらに、通常の磁気抵抗効果より大きな磁
気抵抗変化率を示す伝導電子のスピン依存散乱を利用し
た巨大磁気抵抗効果膜(GMR膜)が開発され、それを
用いたGMRヘッドの一つとして、スピンバルブ構造を
用いたヘッドが提案されている。例えば、特開平4−3
58310号公報参照のこと。
Further, a giant magnetoresistive film (GMR film) utilizing spin-dependent scattering of conduction electrons exhibiting a larger magnetoresistance change rate than a normal magnetoresistive effect has been developed. A head using a spin valve structure has been proposed. For example, Japanese Unexamined Patent Publication No.
See No. 58310.

【0006】スピンバルブは、基本的に第一の強磁性
層、非磁性層、第二の強磁性層、反強磁性層の4層から
なり、交換相互作用が働かない程度に厚い膜厚の非磁性
層を挟んで2つの強磁性層が配置された構造となってい
る。第二の強磁性体層は反強磁性体との交換結合を利用
することで磁化が一方向に固定されており、固定層と呼
ばれる。第一の強磁性層の磁化は外部磁界に対して自由
に回転することができ、自由層と呼ばれる。
The spin valve is basically composed of four layers of a first ferromagnetic layer, a non-magnetic layer, a second ferromagnetic layer, and an antiferromagnetic layer. It has a structure in which two ferromagnetic layers are arranged with a non-magnetic layer interposed therebetween. The magnetization of the second ferromagnetic layer is fixed in one direction by utilizing exchange coupling with an antiferromagnetic substance, and is called a fixed layer. The magnetization of the first ferromagnetic layer can rotate freely with respect to an external magnetic field and is called a free layer.

【0007】このような構造に外部磁界が印加される
と、固定層は磁化の方向を維持し、自由層は外部磁界の
方向に回転する。その結果、2つの強磁性層の相対的な
磁化の向きが変化し、伝導電子のスピン依存散乱が変化
して、磁気抵抗が変化する。
When an external magnetic field is applied to such a structure, the fixed layer maintains the direction of magnetization, and the free layer rotates in the direction of the external magnetic field. As a result, the relative magnetization directions of the two ferromagnetic layers change, the spin-dependent scattering of conduction electrons changes, and the magnetoresistance changes.

【0008】外部磁界に対して自由に回転する層には、
パーマロイ膜等のソフト性の高い薄膜を用いて感度の向
上を図られており、最も実用的な構造と言える。
[0008] In a layer that freely rotates with respect to an external magnetic field,
The sensitivity is improved by using a thin film having high softness such as a permalloy film, and it can be said that this is the most practical structure.

【0009】ところで、薄膜磁気ヘッドの生産性を向上
させるために図8に示すような構造が考えられている。
図8は薄膜磁気ヘッドのヘッド部の拡大断面図をであ
る。
Incidentally, a structure as shown in FIG. 8 has been considered to improve the productivity of the thin film magnetic head.
FIG. 8 is an enlarged sectional view of the head portion of the thin-film magnetic head.

【0010】図8に示す薄膜磁気ヘッドの構造は、スラ
イダー形状にエッチングされたSi単結晶基板101上
に、例えばFeAlSiのような硬度の高い材料からな
る下部シールド層102、例えばSiO2からなる絶縁
層103、上部シールド層104が形成され、絶縁層1
03内にはGMR膜105が形成されている。これが再
生ヘッドである。さらに、上部シールド層102は記録
ヘッド用の下部コアとして共用され、絶縁層106、記
録コイル107、上部コア108からなる記録ヘッドを
構成する。
The structure of the thin film magnetic head shown in FIG. 8 is such that a lower shield layer 102 made of a material having high hardness such as FeAlSi, for example, an insulating material made of SiO 2 is formed on an Si single crystal substrate 101 etched in a slider shape. The layer 103 and the upper shield layer 104 are formed.
The GMR film 105 is formed in the substrate 03. This is the reproducing head. Further, the upper shield layer 102 is commonly used as a lower core for a recording head, and constitutes a recording head including an insulating layer 106, a recording coil 107, and an upper core 108.

【0011】図8の薄膜磁気ヘッドでは、基板にはSi
の単結晶を用い、異方性エッチングによる傾斜面をギャ
ップ深さ方向に使用することで、スライダー形状に加工
するプロセスにおいて、基板を分断することなく最終形
状まで加工を行うことができるため、製造プロセスの大
幅な簡略化を図ることができる。この構造では、磁気抵
抗効果膜は異方性エッチングにより形成される傾斜面上
に形成されることになる。
In the thin-film magnetic head shown in FIG.
By using a single crystal of the above and using an inclined plane by anisotropic etching in the gap depth direction, in the process of processing into a slider shape, it is possible to process to the final shape without dividing the substrate, so manufacturing The process can be greatly simplified. In this structure, the magnetoresistive film is formed on an inclined surface formed by anisotropic etching.

【0012】ところが磁気抵抗効果膜を構成するパーマ
ロイなどの強磁性膜を傾斜面上に形成した場合、斜め入
射の効果により大きな異方性磁界が発生するため、上述
したスピンバルブ膜の磁界感度が大幅に低下するという
問題が生じる。また、スピンバルブ膜において、成膜時
には固定層の異方性の向きを自由層と異方性の向きと直
交させるように最大傾斜線の方向に磁界を印加するが、
斜め入射により発生する異方性が大きいと、強磁性膜の
磁化が磁界の方向を向かないために交換結合が生じない
という問題がある。
However, when a ferromagnetic film such as permalloy forming a magnetoresistive film is formed on an inclined surface, a large anisotropic magnetic field is generated due to the oblique incidence effect. The problem of drastic reduction occurs. In the spin valve film, a magnetic field is applied in the direction of the maximum inclination line so that the direction of the anisotropy of the fixed layer is perpendicular to the direction of the anisotropy of the free layer at the time of film formation.
If the anisotropy generated by oblique incidence is large, there is a problem that exchange coupling does not occur because the magnetization of the ferromagnetic film does not point in the direction of the magnetic field.

【0013】平面上のパーマロイ膜の軟磁気特性の改善
の手段として、TRANSACTION ON MAGNETICS VOL.MAG-15
NO.6 NOVEMBER 1979 「STRUCTURE-SENSITIVE MAG
NETIC PROPERTIES OF RF SPUTTERED NiFe FILMS」に成
膜時に負の直流基板バイアス電圧を印加する方法が記載
されている。これはRFスパッタ法で、Si基板上に4
000Åのパーマロイ膜を形成したものである。−60
〜−120Vの負の直流基板バイアス電圧を印加するこ
とにより、垂直磁気異方性の発生が妨げられ、異方性磁
界5Oeの良好な軟磁気特性を得られるというものであ
る。
As a means for improving the soft magnetic properties of a permalloy film on a plane, TRANSACTION ON MAGNETICS VOL.MAG-15
NO.6 NOVEMBER 1979 `` STRUCTURE-SENSITIVE MAG
"NETIC PROPERTIES OF RF SPUTTERED NiFe FILMS" describes a method of applying a negative DC substrate bias voltage during film formation. This is an RF sputtering method, in which 4
A 2,000 mm permalloy film was formed. -60
By applying a negative DC substrate bias voltage of -120 V, the generation of perpendicular magnetic anisotropy is prevented, and good soft magnetic characteristics with an anisotropic magnetic field of 5 Oe can be obtained.

【0014】また、傾斜面上のパーマロイ膜の軟磁気特
性の改善の手段としては、特開昭61−283107号
公報に、ターゲット電圧とターゲット電流を独立に制御
し得るスパッタリング法において不活性ガス圧およびタ
ーゲット電圧を、パーマロイ膜の保磁力が急峻に立ち上
がるしきい値以上に設定し、かつ、膜が形成される基板
に負のバイアス電圧を印加することにより、傾斜部分の
軟磁気特性の劣化を防ぐことが記載されている。
As a means for improving the soft magnetic characteristics of a permalloy film on an inclined surface, Japanese Patent Application Laid-Open No. 61-283107 discloses an inert gas pressure in a sputtering method capable of controlling a target voltage and a target current independently. By setting the target voltage at or above the threshold value at which the coercive force of the permalloy film rises sharply and applying a negative bias voltage to the substrate on which the film is formed, deterioration of the soft magnetic characteristics of the inclined portion can be prevented. It is stated to prevent.

【0015】[0015]

【発明が解決しようとする課題】スピンバルブ膜に用い
られる強磁性膜の膜厚は100Å以下と非常に薄く、直
流基板バイアス電圧を膜に有効に印加するためには、導
電性の基板又は下地膜上に強磁性膜を形成する必要があ
る。
The thickness of a ferromagnetic film used as a spin valve film is very thin, less than 100 °. In order to effectively apply a DC substrate bias voltage to the film, a conductive substrate or a lower substrate must be used. It is necessary to form a ferromagnetic film on the ground film.

【0016】傾斜面上でTa100Åの下地膜上にパー
マロイ膜100Åを形成した場合の、パーマロイ膜の異
方性磁界Hkの直流基板バイアス電圧依存性を図9に示
す。負の基板バイアス電圧を印加することによってパー
マロイ膜の異方性磁界は減少するが、成膜面が水平面内
にある場合の異方性磁界と比較すると非常に大きい。こ
れは図10に示すようにパーマロイ膜厚が薄くなるほ
ど、大きな異方性磁界が発生することによると考えられ
る。
FIG. 9 shows the DC substrate bias voltage dependence of the anisotropic magnetic field Hk of the permalloy film when the permalloy film 100 # is formed on the Ta100 # underlying film on the inclined surface. The application of a negative substrate bias voltage reduces the anisotropic magnetic field of the permalloy film, but is much larger than the anisotropic magnetic field when the film formation surface is in a horizontal plane. This is presumably because the smaller the permalloy film thickness, the larger the anisotropic magnetic field is generated, as shown in FIG.

【0017】また、直流基板バイアス電圧を印加した場
合、電荷の集中のためか、バイアスの絶対値を大きくし
ていくと斜面のターゲットに近い側の膜厚が極端に減少
してしまうという問題が生じる。
Also, when a DC substrate bias voltage is applied, there is a problem that the film thickness on the side closer to the target on the slope is extremely reduced if the absolute value of the bias is increased, probably because of the concentration of charges. Occurs.

【0018】形成されるパーマロイ膜の膜厚が十分大き
ければ、ある程度膜厚が形成された後はバイアスが印加
されることになり、導電性の下地膜を形成しなくとも基
板バイアス電圧印加の効果を得ることができると思われ
るが、膜厚が100Å以下と薄い場合は難しい。
If the thickness of the permalloy film to be formed is sufficiently large, a bias is applied after the film is formed to a certain extent, and the effect of applying the substrate bias voltage can be obtained without forming a conductive base film. However, when the film thickness is as thin as 100 ° or less, it is difficult.

【0019】このように、傾斜面上にスピンバルブ膜に
用いられるような薄いパーマロイ膜を形成する場合、上
記のように直流基板バイアス電圧を印加することでは、
平面上と同等の軟磁気特性は得られない。
As described above, when a thin permalloy film used for a spin valve film is formed on an inclined surface, by applying a DC substrate bias voltage as described above,
Soft magnetic characteristics equivalent to those on a plane cannot be obtained.

【0020】このように、磁気抵抗効果膜を構成する強
磁性膜を傾斜面上に形成した場合、斜め入射の効果によ
り大きな異方性磁界が発生するため、上述したスピンバ
ルブ膜の磁界感度が大幅に低下するという問題が生じ
る。また、スピンバルブ膜において、成膜時に固定層の
異方性の向きを自由層の異方性の向きと直交させるよう
に、最大傾斜線の方向に磁界を印加するが、斜め入射に
より発生する異方性が大きいと強磁性膜の磁化が磁界の
方向を向かないため、交換結合が生じないという問題が
生じる。
As described above, when the ferromagnetic film constituting the magnetoresistive effect film is formed on the inclined surface, a large anisotropic magnetic field is generated due to the oblique incidence effect. The problem of drastic reduction occurs. In the spin valve film, a magnetic field is applied in the direction of the maximum inclination line so that the direction of the anisotropy of the fixed layer is perpendicular to the direction of the anisotropy of the free layer at the time of film formation. If the anisotropy is large, the magnetization of the ferromagnetic film does not point in the direction of the magnetic field, so that there is a problem that exchange coupling does not occur.

【0021】本発明の目的は、スパッタリング法におい
て、磁気抵抗効果膜が被着される成膜面の少なくとも一
部がターゲットに平行な面から傾いている関係を有する
場合に、被着される強磁性膜の膜厚がスピンバルブ膜に
用いられるような薄い場合でも、高い感度と大きな交換
結合磁界が得られる磁気抵抗効果膜が得られる磁気抵抗
効果膜の製造方法、それを用いた磁気抵抗効果膜、並び
に薄膜磁気ヘッドを提供することにある。
An object of the present invention is to provide a sputtering method in which at least a part of a deposition surface on which a magnetoresistive film is deposited has a relationship inclined from a plane parallel to a target. A method of manufacturing a magnetoresistive film capable of obtaining a magnetoresistive film capable of obtaining a high sensitivity and a large exchange coupling magnetic field even when the thickness of the magnetic film is as thin as that used for a spin valve film, and a magnetoresistive effect using the same. A thin film magnetic head is provided.

【0022】[0022]

【課題を解決するための手段】本発明は上記目的を達成
させるためになされたものであって、請求項1記載の発
明は、スパッタ法を用いて、少なくとも第1の強磁性
層、非磁性層、第2の強磁性層、反強磁性層から構成さ
れる磁気抵抗効果膜を、ターゲット面に対して一部分が
傾いた基板上に形成する磁気抵抗効果膜の製造方法であ
って、 少なくとも第1の強磁性層の成膜中に、前記基
板に高周波バイアスを印加することを特徴とする磁気抵
抗効果膜の製造方法である。
SUMMARY OF THE INVENTION The present invention has been made to achieve the above object, and the invention according to claim 1 uses at least a first ferromagnetic layer and a non-magnetic layer by sputtering. A method of forming a magnetoresistive film comprising a layer, a second ferromagnetic layer, and an antiferromagnetic layer on a substrate partially inclined with respect to a target surface, comprising: A method of manufacturing a magnetoresistive film, wherein a high-frequency bias is applied to the substrate during the formation of one ferromagnetic layer.

【0023】また、請求項2記載の発明は、前記ターゲ
ットと前記基板のなす角度が略55°であり、且つ高周
波バイアスの電力がターゲットへの投入電力の4%以上
であることを特徴とする請求項1記載の磁気抵抗効果膜
の製造方法である。
Further, the invention according to claim 2 is characterized in that the angle between the target and the substrate is approximately 55 °, and the power of the high frequency bias is 4% or more of the power applied to the target. A method for manufacturing a magnetoresistive film according to claim 1.

【0024】また、請求項3記載の発明は、前記磁気抵
抗効果膜を、非晶質基板または非晶質膜が成膜された基
板上に形成することを特徴とする請求項1または2記載
の磁気抵抗効果膜の製造方法である。
According to a third aspect of the present invention, the magnetoresistance effect film is formed on an amorphous substrate or a substrate on which the amorphous film is formed. This is a method for manufacturing a magnetoresistive film.

【0025】また、請求項4記載の発明は、前記請求項
1乃至3記載の製造方法により製造されたことを特徴と
する磁気抵抗効果膜である。
According to a fourth aspect of the present invention, there is provided a magnetoresistive film manufactured by the manufacturing method according to the first to third aspects.

【0026】また、請求項5記載の発明は、前記請求項
4記載の磁気抵抗効果膜を有する薄膜磁気ヘッドであ
る。
According to a fifth aspect of the present invention, there is provided a thin film magnetic head having the magnetoresistive effect film according to the fourth aspect.

【0027】[0027]

【発明の実施の形態】以下、図をもとに本発明について
説明する。なお、これによって本発明は限定されるもの
ではない。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below with reference to the drawings. Note that the present invention is not limited by this.

【0028】ここでは、傾斜面上に形成された磁気抵抗
効果膜の特性を簡便に調べるために、単純な配置のモデ
ルを使用した。そのモデルを図1に示す。ターゲット2
は水平面内に設置され、磁気抵抗効果膜が被着される成
膜面3(基板1)は水平面から傾いており、ターゲット
2と成膜面3(基板1)の成す角度は略55°である。
このような配置において各膜を形成した。
Here, in order to easily check the characteristics of the magnetoresistive film formed on the inclined surface, a model having a simple arrangement was used. The model is shown in FIG. Target 2
Is disposed in a horizontal plane, the deposition surface 3 (substrate 1) on which the magnetoresistive effect film is deposited is inclined from the horizontal plane, and the angle between the target 2 and the deposition surface 3 (substrate 1) is approximately 55 °. is there.
Each film was formed in such an arrangement.

【0029】ここで、角度を略55°としたのは、後述
する実施例3で説明する薄膜ヘッドにおいて成膜面と水
平面がなす角度が略55°であることから選ばれてい
る。しかし、本発明による異方性磁界低減の効果は、特
別な角度に限られるものではなく、高周波基板バイアス
の電力を適当に設定することで同様な効果を得ることが
できる。
Here, the reason why the angle is set to approximately 55 ° is selected because the angle formed between the film forming surface and the horizontal plane in the thin film head described in the third embodiment described later is approximately 55 °. However, the effect of reducing the anisotropic magnetic field according to the present invention is not limited to a special angle, and the same effect can be obtained by appropriately setting the power of the high-frequency substrate bias.

【0030】また、磁気抵抗効果膜が実際の磁気ヘッド
のパターン上に形成された場合にも、このモデルにより
得られた結果と同様の結果を得ることができる。
Further, even when the magnetoresistive film is formed on the actual pattern of the magnetic head, the same result as that obtained by this model can be obtained.

【0031】[実施例1]以下、実施例1について説明
する。
[Embodiment 1] Hereinafter, Embodiment 1 will be described.

【0032】図1に示すモデルを用いてパーマロイ膜を
形成した。膜の構成は基板1をガラス基板(コーニング
社製:#7059)とし、成膜にはロードロック室を備
える多元スパッタ装置を用い、プロセスチャンバーを5
×10-8Torr以下まで排気した後、同一真空中で下
地層のTa膜、軟磁性体層のパーマロイ膜を順に形成し
ている。
A permalloy film was formed using the model shown in FIG. The structure of the film was such that the substrate 1 was a glass substrate (Corning: # 7059), a multi-source sputtering apparatus having a load lock chamber was used for film formation, and the process chamber was 5
After evacuation to × 10 −8 Torr or less, a Ta film as a base layer and a Permalloy film as a soft magnetic layer are formed in this order in the same vacuum.

【0033】Ta膜、パーマロイ膜はともにRFコンベ
ンショナルスパッタ法にて、Arガス圧:5mTorr
のもとで、Ta膜はPower:100W、パーマロイ
膜は250Wでともに100Åの膜厚で成膜した。
Both the Ta film and the permalloy film were formed by RF conventional sputtering using an Ar gas pressure of 5 mTorr.
The Ta film was formed at a power of 100 W and the Permalloy film was formed at a thickness of 100 W at 250 W.

【0034】本実施例ではパーマロイ膜の成膜にRFコ
ンベンショナルスパッタ法を用いたが、他にRFマグネ
トロンスパッタ法、DCマグネトロンスパッタ法などの
一般のスパッタリング法を用いることができる。
In this embodiment, the RF conventional sputtering method is used for forming the permalloy film, but other general sputtering methods such as an RF magnetron sputtering method and a DC magnetron sputtering method can be used.

【0035】図2に上記のTa下地膜に形成されたパー
マロイ膜の異方性磁界Hkの高周波基板バイアス依存性
を示す。
FIG. 2 shows the dependency of the anisotropic magnetic field Hk of the permalloy film formed on the Ta underlayer on the high-frequency substrate bias.

【0036】図2に示すように、高周波基板バイアスを
印加することによって異方性磁界は減少している。高周
波バイアスの電力が10W以上で異方性磁界は大きく減
少しているが、これはターゲットへの投入電力の4%に
相当する。高周波基板バイアス100Wの印加で異方性
磁界は65Oe程度まで低下しており、負の直流基板バ
イアス電圧を印加した場合より、効果が大きい。しかも
直流基板バイアスの場合とは異なり、膜厚分布はほとん
ど生じていない。
As shown in FIG. 2, the anisotropic magnetic field is reduced by applying a high-frequency substrate bias. When the power of the high frequency bias is 10 W or more, the anisotropic magnetic field is greatly reduced, which corresponds to 4% of the power supplied to the target. The application of a high-frequency substrate bias of 100 W reduces the anisotropic magnetic field to about 65 Oe, which is more effective than when a negative DC substrate bias voltage is applied. Further, unlike the case of the DC substrate bias, the film thickness distribution hardly occurs.

【0037】このようにパーマロイ膜を形成する際に、
成膜時に高周波基板バイアスを印加することで、水平か
ら傾斜した面上においても軟磁気特性の劣化を防ぐこと
ができる。
When a permalloy film is formed as described above,
By applying a high-frequency substrate bias during film formation, deterioration of soft magnetic characteristics can be prevented even on a surface inclined from horizontal.

【0038】なお、印加される最適の高周波基板バイア
スの値は、基板の角度、成膜チャンバーの大きさ等によ
り適当に設定することができる。
The optimum value of the applied high-frequency substrate bias can be appropriately set depending on the angle of the substrate, the size of the film forming chamber, and the like.

【0039】また、上記の例ではスパッタリングターゲ
ットとしてNiFeの二元パーマロイ合金を使用してい
るが、Mo、Ti、Cr、V、Nbが添加された合金を
用いても同様の効果を得ることができる。
In the above example, a binary permalloy of NiFe is used as the sputtering target, but the same effect can be obtained by using an alloy to which Mo, Ti, Cr, V, and Nb are added. it can.

【0040】次に、このようにして得られるパーマロイ
膜を用いて、磁気抵抗効果膜(スピンバルブ膜)を作成
した。
Next, a magnetoresistive film (spin valve film) was formed using the permalloy film thus obtained.

【0041】図4は本実施例の形態のスピンバルブ膜の
構成を示す概略図である。基板としてガラス基板(コー
ニング社製:#7059)41、自由層として100Å
のパーマロイ膜4と7ÅのCo膜5の積層膜、非磁性層
として32ÅのCu膜6、固定層としての10ÅのCo
膜7、50Åのパーマロイ膜8及び5ÅのCo膜9の積
層膜、反強磁性体層として200ÅのPtMn合金膜1
0、保護層として100ÅのTa膜11を用いた。
FIG. 4 is a schematic view showing the structure of the spin valve film according to this embodiment. A glass substrate (Corning Co .: # 7059) 41 as a substrate, and a free layer of 100 mm
Laminated film of a permalloy film 4 and a Co film 5 of 7%, a Cu film 6 of 32% as a nonmagnetic layer, and a Co film of 10% as a fixed layer.
Film 7, a laminated film of a permalloy film 8 of 50 ° and a Co film 9 of 5 °, and a PtMn alloy film 1 of 200 ° as an antiferromagnetic layer
0, a 100 ° Ta film 11 was used as a protective layer.

【0042】このとき反強磁性体層となるPtMn合金
の成膜には、Mnターゲット上にPtペレットを配置し
た複合ターゲットを用い、Ptの組成は47.4原子%
とした。
At this time, for forming a PtMn alloy to be an antiferromagnetic layer, a composite target in which Pt pellets are arranged on a Mn target is used, and the composition of Pt is 47.4 atomic%.
And

【0043】本実施例では反強磁性体としてPtMn合
金を用いたが、他にRuMn、IrMn、PtMnなど
のγ−Mn系合金、または、規則層を持つ反強磁性体と
して、NiMn合金、PdMn合金、PdMnPt合金
などを用いることもできる。しかし、γ−Mn系合金を
用いた場合の交換結合磁界は結晶性、配向に敏感なた
め、大きな交換結合磁界を得るためには、結晶性を向上
させるTa等の下地膜を必要とするので、Hkの低下に
限界があり、結晶性、配向に鈍感な規則層を持つ反強磁
性体のほうが望ましい。さらにその中でも、交換結合磁
界の大きさ、耐食性、交換結合磁界を発生するための熱
処理温度と時間などの観点から判断すると、PtMn合
金が総合的にすぐれている。
In this embodiment, a PtMn alloy was used as the antiferromagnetic material. However, a γ-Mn alloy such as RuMn, IrMn, and PtMn, or a NiMn alloy, PdMn as an antiferromagnetic material having an ordered layer is also used. An alloy, a PdMnPt alloy, or the like can also be used. However, since the exchange coupling magnetic field when a γ-Mn alloy is used is sensitive to crystallinity and orientation, in order to obtain a large exchange coupling magnetic field, a base film such as Ta for improving crystallinity is required. , Hk is limited, and an antiferromagnetic material having a regular layer insensitive to crystallinity and orientation is more preferable. Among them, the PtMn alloy is generally superior in terms of the magnitude of the exchange coupling magnetic field, corrosion resistance, and the heat treatment temperature and time for generating the exchange coupling magnetic field.

【0044】本実施例では成膜にロードロック室を備え
る多元スパッタ装置を用い、プロセスチャンバーを5×
10-8Torr以下まで排気した後、すべての層を同一
真空中で形成した。
In this embodiment, a multi-source sputtering apparatus having a load lock chamber for film formation is used, and the process chamber is set to 5 ×
After evacuation to 10 -8 Torr or less, all layers were formed in the same vacuum.

【0045】次に、パーマロイ膜、Co膜、Cu膜、P
tMn合金膜、Ta膜の成膜方法、および成膜条件につ
いて説明する。
Next, a permalloy film, a Co film, a Cu film, P
The method for forming the tMn alloy film and the Ta film and the film forming conditions will be described.

【0046】パーマロイ膜、Co膜、Ta膜はRFコン
ベンショナルスパッタ法にて成膜し、Powerはそれ
ぞれ250W、150W、100Wとした。また、パー
マロイ膜の成膜時には、高周波基板バイアス30Wを印
加している。Cu膜、MnPt合金膜はDCマグネトロ
ンスパッタ法にて成膜し、Powerは40Wとした。
なお、成膜時のArガス圧はすべて5mTorrでおこ
なっている。
The permalloy film, the Co film, and the Ta film were formed by RF conventional sputtering, and the power was 250 W, 150 W, and 100 W, respectively. In forming the permalloy film, a high-frequency substrate bias of 30 W is applied. The Cu film and the MnPt alloy film were formed by DC magnetron sputtering, and the power was 40 W.
Note that the Ar gas pressure during film formation is all set at 5 mTorr.

【0047】その後、得られたスピンバルブ膜につい
て、PtMn合金膜の規則合金化のために、300Oe
の磁界中で250℃、6時間の熱処理を行った。PtM
n合金膜の規則合金化は200℃程度から始まり、それ
にともなって、交換結合磁界も発生するが、十分な規則
化を進めるためには230℃以上で行うことが望まし
い。
Thereafter, the obtained spin valve film was subjected to 300 Oe for orderly alloying the PtMn alloy film.
In a magnetic field of 250 ° C. for 6 hours. PtM
The ordered alloying of the n-alloy film starts at about 200 ° C., and accordingly, an exchange coupling magnetic field is generated. However, it is desirable to perform the alloying at 230 ° C. or higher in order to promote sufficient ordering.

【0048】また、固定層および自由層は、成膜中に面
内の互いに直交する方向に、50Oeの磁界を印加しな
がら形成している。
The fixed layer and the free layer are formed while applying a magnetic field of 50 Oe in a direction perpendicular to each other in the plane during the film formation.

【0049】なお、上記の磁気抵抗効果膜における自由
層、固定層はパーマロイ膜とCo合金膜から構成されて
いる。このように、パーマロイ膜とCu膜の間に若干の
Coを挿入することで抵抗変化率が増加する、あるいは
パーマロイ膜とCu膜の拡散防止の効果によりスピンバ
ルブ膜の耐熱性が向上する効果がある。また、反強磁性
層とパーマロイ膜との間にCoを挿入することで、その
交換結合磁界を増大することができる。その際、Co膜
はパーマロイ膜に比べて薄いため、磁気特性に対してほ
とんど影響をおよぼさない。
The free layer and the fixed layer in the above-mentioned magnetoresistive film are made of a permalloy film and a Co alloy film. As described above, by inserting a small amount of Co between the permalloy film and the Cu film, the resistance change rate increases, or the effect of preventing the diffusion of the permalloy film and the Cu film improves the heat resistance of the spin valve film. is there. Further, by inserting Co between the antiferromagnetic layer and the permalloy film, the exchange coupling magnetic field can be increased. At this time, since the Co film is thinner than the Permalloy film, it hardly affects the magnetic characteristics.

【0050】このようにして得られたスピンバルブ膜の
磁化曲線を図4に示す。自由層の異方性磁界は70Oe
まで減少し、直流バイアスを印加した場合に比べて、自
由層の軟磁気特性は改善されている。
FIG. 4 shows the magnetization curve of the spin valve film obtained in this manner. The anisotropic magnetic field of the free layer is 70 Oe
The soft magnetic characteristic of the free layer is improved as compared with the case where a DC bias is applied.

【0051】したがって、本発明により、斜め入射の効
果により発生する大きな異方性磁界が低減され、スピン
バルブ構造を持つ磁気抵抗効果膜の磁界感度の低下を防
止することができる。また、素子の安定性に必要な大き
な交換結合磁界も得ることができる。
Therefore, according to the present invention, a large anisotropic magnetic field generated by the effect of oblique incidence is reduced, and a decrease in the magnetic field sensitivity of the magnetoresistive film having the spin valve structure can be prevented. Also, a large exchange coupling magnetic field required for the stability of the element can be obtained.

【0052】したがって、このようにして得られる磁気
抵抗効果膜を用いれば、磁気抵抗効果膜が傾斜面上に形
成される形態の薄膜磁気ヘッドにおいても高い磁界感度
と素子の安定性を得ることができる。
Therefore, if the magnetoresistive film thus obtained is used, high magnetic field sensitivity and element stability can be obtained even in a thin film magnetic head in which the magnetoresistive effect film is formed on an inclined surface. it can.

【0053】[実施例2]以下、実施例2について説明
する。
Embodiment 2 Hereinafter, Embodiment 2 will be described.

【0054】本実施例では、Al2O3膜上に磁気抵抗効
果膜を形成した。Al2O3膜の成膜にはRFマグネトロ
ンスパッタ装置を用い、ガラス基板(コーニング社製:
#7059)上に、Arガス圧:5mTorr、基板水
冷、Power:400W、高周波基板バイアス50W
の条件にて行った。膜厚は1300Åである。
In this embodiment, a magnetoresistive film was formed on the Al 2 O 3 film. An RF magnetron sputtering apparatus was used for forming the Al 2 O 3 film, and a glass substrate (manufactured by Corning:
# 7059) Ar gas pressure: 5 mTorr, substrate water cooling, Power: 400 W, high frequency substrate bias 50 W
Was performed under the following conditions. The film thickness is 1300 °.

【0055】このようにして得られたAl2O3膜上に実
施例1と同様の方法で、パーマロイ膜を形成した。
A permalloy film was formed on the Al 2 O 3 film thus obtained in the same manner as in Example 1.

【0056】図5に上記のAl2O3下地膜に形成された
パーマロイ膜の異方性磁界Hkの高周波基板バイアス依
存性を示す。
FIG. 5 shows the dependency of the anisotropic magnetic field Hk of the permalloy film formed on the Al 2 O 3 underlayer on the high-frequency substrate bias.

【0057】図5に示すように、高周波基板バイアスを
印加することによって異方性磁界は減少している。30
Wで異方性磁界は6.5Oeまで低下し、成膜面が水平
面内にある場合とほぼ同じの良好な軟磁気特性が得られ
ている。本実施例では、下地膜としてAl2O3膜を用い
たがSiO2などの他の非晶質膜、または、ガラスなど
非晶質基板を用いることもできる。このように、非晶質
膜、または、非晶質基板上にパーマロイ膜を形成するこ
とで、さらに軟磁気特性に優れたパーマロイ膜を得るこ
とができる。
As shown in FIG. 5, the anisotropic magnetic field is reduced by applying a high-frequency substrate bias. 30
At W, the anisotropic magnetic field is reduced to 6.5 Oe, and the same good soft magnetic characteristics as when the film forming surface is in the horizontal plane are obtained. In this embodiment, an Al 2 O 3 film is used as a base film. However, another amorphous film such as SiO 2 or an amorphous substrate such as glass can be used. Thus, by forming a permalloy film on an amorphous film or an amorphous substrate, a permalloy film having more excellent soft magnetic characteristics can be obtained.

【0058】非晶質基板または非晶質膜上で異方性磁界
が低下する原因は次のように考えられる。例えば、パー
マロイ膜を平面上の基板に形成する場合、Ta下地上に
成膜すると結晶性の良い膜ができるが、ガラス基板上又
はAl2O3、SiO2などの非晶質基板上に成膜すると
結晶性はあまり良くない。これはX線回折の(111)
面の回折強度から知ることができる。
The cause of the decrease in the anisotropic magnetic field on the amorphous substrate or the amorphous film is considered as follows. For example, when a permalloy film is formed on a flat substrate, a film having good crystallinity can be formed by forming the film on a Ta base, but the film is formed on a glass substrate or an amorphous substrate such as Al 2 O 3 or SiO 2. The crystallinity is not very good when filmed. This is the X-ray diffraction (111)
It can be known from the diffraction intensity of the surface.

【0059】このことから、斜面上でも非晶質基板又は
非晶質の下地膜上にパーマロイ膜を形成すると、斜め入
射により生じる特有の膜構造の形成が起こりにくくな
り、異方性磁界が低下するのではないかと考えられる。
したがって、本発明のように非晶質の下地膜上に高周波
バイアスを用いて成膜することにより、形成されるパー
マロイ膜が非常に薄い場合でも、平面上に形成された場
合と同等の軟磁気特性が得られることができる。
Therefore, when a permalloy film is formed on an amorphous substrate or an amorphous base film even on a slope, it is difficult to form a unique film structure caused by oblique incidence, and the anisotropic magnetic field is reduced. It is thought that we may do it.
Therefore, even when the permalloy film to be formed is extremely thin by forming a film on an amorphous base film using a high-frequency bias as in the present invention, the soft magnetic property is equivalent to that when the film is formed on a flat surface. Properties can be obtained.

【0060】このようにして得られたスピンバルブ膜の
磁化曲線を図6に示す。自由層の磁化は微少な印加磁界
で急激に立ち上がっており、成膜面3が水平面内にある
場合と同等の良好な軟磁気特性が得られている。したが
って、本発明により、斜め入射の効果により発生する大
きな異方性磁界が低減され、スピンバルブ構造を持つ磁
気抵抗効果膜の磁界感度の低下を防止することができ
る。また、素子の安定性に必要な大きな交換結合磁界も
得ることができる。
FIG. 6 shows the magnetization curve of the spin valve film thus obtained. The magnetization of the free layer rises sharply with a very small applied magnetic field, and good soft magnetic characteristics equivalent to the case where the film formation surface 3 is in a horizontal plane are obtained. Therefore, according to the present invention, a large anisotropic magnetic field generated by the effect of oblique incidence is reduced, and a decrease in the magnetic field sensitivity of the magnetoresistive film having the spin valve structure can be prevented. Also, a large exchange coupling magnetic field required for the stability of the element can be obtained.

【0061】したがって、このようにして得られる磁気
抵抗効果膜を用いれば、磁気抵抗効果膜が傾斜面上に形
成される形態の薄膜磁気ヘッドにおいても高い磁界感度
と素子の安定性を得ることができる。
Therefore, by using the magnetoresistive film thus obtained, high magnetic field sensitivity and element stability can be obtained even in a thin film magnetic head in which the magnetoresistive effect film is formed on an inclined surface. it can.

【0062】[実施例3]以下、実施例3について説明
する。
Embodiment 3 Hereinafter, Embodiment 3 will be described.

【0063】本発明における磁気ディスク装置に用いら
れる薄膜磁気ヘッドの断面図を図7に示す。この様な薄
膜磁気ヘッドは以下のように作成することができる。
FIG. 7 is a sectional view of a thin-film magnetic head used in the magnetic disk drive according to the present invention. Such a thin film magnetic head can be manufactured as follows.

【0064】まず、(100)面12を表面とするSi
単結晶基板13上にレジストパターンを形成し、KO
H、NaOH等のエッチング液を用いて所定のスライダ
ー形状にエッチングを行う。このとき、エッチング深さ
方向の断面にはSiの(111)面14が露出する。
(111)面の斜面の角度は結晶方位によって決定され
るため、略55°となる。この角度は結晶面の傾きであ
るので常に精度良く、また非常に平滑な斜面を形成する
ことができる。
First, the Si having the (100) plane 12 as the surface
A resist pattern is formed on the single crystal substrate 13 and KO
Etching is performed in a predetermined slider shape using an etchant such as H or NaOH. At this time, the (111) plane 14 of Si is exposed in the cross section in the etching depth direction.
Since the angle of the slope of the (111) plane is determined by the crystal orientation, it is approximately 55 °. Since this angle is the inclination of the crystal plane, an extremely smooth slope can always be formed with high accuracy.

【0065】次に当該基板13上に、下部シールド15
層を形成する。本発明では上記基板の材料はSiである
ので、特に硬度の高い材料を必要とせず、パーマロイ膜
の使用が可能である。このため、メッキ法の使用が可能
であり、傾斜面の磁気特性の制御ができる。
Next, the lower shield 15 is placed on the substrate 13.
Form a layer. In the present invention, since the material of the substrate is Si, a material having a particularly high hardness is not required, and a permalloy film can be used. For this reason, the plating method can be used, and the magnetic characteristics of the inclined surface can be controlled.

【0066】次に上記下部シールド層15上に絶縁層を
形成するが、Al2O3膜またはSiO2膜を用いること
ができる。
Next, an insulating layer is formed on the lower shield layer 15, and an Al 2 O 3 film or a SiO 2 film can be used.

【0067】次に磁気抵抗効果膜を形成する。これには
実施例2に用いたスピンバルブ膜を使用する。
Next, a magnetoresistive film is formed. The spin valve film used in Example 2 is used for this.

【0068】上述したように本発明によれば、アモルフ
ァスの下地膜上に高周波基板バイアス印加して成膜する
ことで良好な軟磁気特性を得ることができるため、スピ
ンバルブ構造を持つ磁気抵抗効果膜の磁界感度の低下を
防止することができる。
As described above, according to the present invention, good soft magnetic characteristics can be obtained by applying a high-frequency substrate bias on an amorphous base film, so that a magnetoresistive effect having a spin valve structure can be obtained. A decrease in the magnetic field sensitivity of the film can be prevented.

【0069】次に上記の磁気抵抗効果膜を所定の形状に
加工し、磁区制御用の高保磁力膜、読み出し用のリード
パターンを形成し、さらに絶縁層を介して上部シールド
層17を形成することで、再生用のヘッドが製造され
る。
Next, the above-mentioned magnetoresistive effect film is processed into a predetermined shape, a high coercive force film for controlling magnetic domains, a read lead pattern are formed, and an upper shield layer 17 is formed via an insulating layer. Thus, a reproducing head is manufactured.

【0070】次に形成される上部シールド17は記録ヘ
ッドのコアと共用されることで、記録ヘッドを構成す
る。まず、ギャップ材としてSiO2等の絶縁層が形成
される。次に記録用のコイル18としてCu膜を形成す
る。当該Cu膜は選択メッキによって形成される。
The upper shield 17 formed next is used in common with the core of the recording head to constitute the recording head. First, an insulating layer such as SiO 2 is formed as a gap material. Next, a Cu film is formed as the recording coil 18. The Cu film is formed by selective plating.

【0071】なお、記録ヘッドにおける絶縁層は通常厚
く形成する必要があり、感光性の有機膜を塗布後、所定
パターンに形成した後、ベーキングを行う。その後、上
部コアをパーマロイのメッキ膜19で形成する。
Incidentally, the insulating layer in the recording head usually needs to be formed thick, and after applying a photosensitive organic film, forming a predetermined pattern, and then performing baking. Thereafter, the upper core is formed of a permalloy plating film 19.

【0072】記録ヘッドについても、磁気ギャップが基
板に対して平行ではなく、略55°傾斜した薄膜磁気ヘ
ッドを形成することができる。
As for the recording head, it is possible to form a thin-film magnetic head in which the magnetic gap is not parallel to the substrate but is inclined at about 55 °.

【0073】以上の様に、基板13上に薄膜磁気ヘッド
を形成した後、基板表面を精密に研磨することにより、
不要なパターンの削除とMR高さと記録ヘッドのギャッ
プ深さを設定する。その後保護、潤滑の目的でDLC
(Diamond LikeCarbon)をCVD法
で形成することで、耐CSS(Contact Sta
rt Stop)特性を得ることができる。以上の様に
本発明の薄膜磁気ヘッドの形態に従い、基板にはSi
の単結晶を用い、異方性エッチングによる傾斜面をギャ
ップ深さ方向に使用することで、スライダー形状に加工
するプロセスにおいて、基板を分断することなく最終形
状まで加工を行うことができるため、製造プロセスの大
幅な簡略化を図ることができる。
As described above, after the thin-film magnetic head is formed on the substrate 13, the substrate surface is precisely polished,
Unnecessary patterns are deleted, and the MR height and the gap depth of the recording head are set. DLC for protection and lubrication
(Diamond Like Carbon) is formed by a CVD method, so that CSS (Contact Sta.
rt Stop) characteristic can be obtained. As described above, according to the embodiment of the thin film magnetic head of the present invention,
By using a single crystal of the above and using an inclined plane by anisotropic etching in the gap depth direction, in the process of processing into a slider shape, it is possible to process to the final shape without dividing the substrate, so manufacturing The process can be greatly simplified.

【0074】さらに、実施例2に述べたスピンバルブ膜
を用いることにより、磁界感度が高く、外乱磁界に対し
て安定な薄膜磁気ヘッドを得ることができる。
Further, by using the spin valve film described in the second embodiment, a thin film magnetic head having high magnetic field sensitivity and stable against a disturbance magnetic field can be obtained.

【0075】[0075]

【発明の効果】本発明によれば、請求項1記載の発明で
は、スパッタ法を用いて、少なくとも第1の強磁性層、
非磁性層、第2の強磁性層、反強磁性層から構成される
磁気抵抗効果膜を、ターゲット面に対して一部分が傾い
た基板上に形成する磁気抵抗効果膜の製造方法であっ
て、少なくとも第1の強磁性層の成膜中に、前記基板に
高周波バイアスを印加すると、平面上に形成された場合
と同等の軟磁気特性が得ることができ、さらに、このよ
うにして得られた強磁性膜を用いることで、感度の高い
スピンバルブ膜を得ることができる。
According to the present invention, according to the first aspect of the present invention, at least the first ferromagnetic layer is formed by sputtering.
A method for manufacturing a magnetoresistive film, comprising: forming a magnetoresistive film including a nonmagnetic layer, a second ferromagnetic layer, and an antiferromagnetic layer on a substrate having a part inclined with respect to a target surface; When a high-frequency bias is applied to the substrate at least during the formation of the first ferromagnetic layer, soft magnetic characteristics equivalent to those formed on a flat surface can be obtained, and furthermore, obtained in this way. By using a ferromagnetic film, a highly sensitive spin valve film can be obtained.

【0076】また、請求項2記載の発明は、前記ターゲ
ットと前記基板のなす角度が略55°であり、且つ高周
波バイアスの電力がターゲットへの投入電力の4%以上
とすると、さらに異方性磁界を大きく減少させることが
できる。
The invention according to claim 2 is further characterized in that the angle between the target and the substrate is approximately 55 ° and the power of the high frequency bias is 4% or more of the power applied to the target. The magnetic field can be greatly reduced.

【0077】また、請求項3記載の発明は、前記磁気抵
抗効果膜を、非晶質基板または非晶質膜が成膜された基
板上に形成すると、さらに異方性磁界を大きく減少させ
ることができる。
According to a third aspect of the present invention, when the magnetoresistance effect film is formed on an amorphous substrate or a substrate on which the amorphous film is formed, the anisotropic magnetic field is further reduced. Can be.

【0078】また、請求項4記載の発明は、前記請求項
1乃至3記載の製造方法により製造されたことを特徴と
する磁気抵抗効果膜であるので、平面上に形成された場
合と同等の軟磁気特性を有し、感度の高いスピンバルブ
膜であり、さらに異方性磁界が大きく減少したスピンバ
ルブ膜である。
The invention according to claim 4 is a magnetoresistive film manufactured by the manufacturing method according to any one of claims 1 to 3, and is equivalent to a film formed on a plane. A spin valve film having soft magnetic characteristics and high sensitivity, and a spin valve film in which an anisotropic magnetic field is greatly reduced.

【0079】また、請求項5記載の発明は、前記請求項
4記載の磁気抵抗効果膜を有する薄膜磁気ヘッドである
ので、水平から傾斜した面にスピンバルブ膜が形成され
る構造の薄膜磁気ヘッドでも、高い磁界感度を維持する
ことができ、製造プロセスの大幅に簡略化された薄膜磁
気ヘッドを得ることができる。
According to a fifth aspect of the present invention, there is provided a thin film magnetic head having the magnetoresistive effect film according to the fourth aspect, so that the thin film magnetic head has a structure in which a spin valve film is formed on a surface inclined from horizontal. However, a high magnetic field sensitivity can be maintained, and a thin-film magnetic head whose manufacturing process is greatly simplified can be obtained.

【0080】また、上述したような薄膜磁気ヘッド以外
にも、ガラスなどの基板上に形成された斜面上に本発明
の磁気抵抗効果膜を形成することで、複数の方向の磁界
を検出する多次元センサーを同一基板上に形成すること
もできる。
In addition to the above-described thin-film magnetic head, by forming the magnetoresistive film of the present invention on a slope formed on a substrate such as glass, it is possible to detect magnetic fields in a plurality of directions. The dimensional sensor can be formed on the same substrate.

【図面の簡単な説明】[Brief description of the drawings]

【図1】基板1とターゲット2との配置のモデル図であ
る。
FIG. 1 is a model diagram of an arrangement of a substrate 1 and a target 2.

【図2】Ta膜上にパーマロイ膜を形成した場合の、異
方性磁界Hkの高周波基板バイアス依存性を示すグラフ
の図である。
FIG. 2 is a graph showing a high frequency substrate bias dependence of an anisotropic magnetic field Hk when a permalloy film is formed on a Ta film.

【図3】スピンバルブ膜の膜構成を示す概略図である。FIG. 3 is a schematic diagram showing a film configuration of a spin valve film.

【図4】スピンバルブ膜の磁化曲線を示す図である。FIG. 4 is a diagram showing a magnetization curve of a spin valve film.

【図5】Al2O3膜上にパーマロイ膜を形成した場合
の、異方性磁界Hkの高周波基板バイアス依存性を示す
グラフの図である。
FIG. 5 is a graph showing the high frequency substrate bias dependence of the anisotropic magnetic field Hk when a permalloy film is formed on an Al 2 O 3 film.

【図6】スピンバルブ膜の磁化曲線を示す図である。FIG. 6 is a diagram showing a magnetization curve of a spin valve film.

【図7】本発明の薄膜磁気ヘッドの断面図である。FIG. 7 is a sectional view of a thin-film magnetic head according to the present invention.

【図8】従来技術の薄膜磁気ヘッドの断面図である。FIG. 8 is a cross-sectional view of a conventional thin-film magnetic head.

【図9】パーマロイ膜の異方性磁界Hkの直流基板バイ
アス電圧依存性を示すグラフの図である。
FIG. 9 is a graph showing the DC substrate bias voltage dependency of the anisotropic magnetic field Hk of the permalloy film.

【図10】異方性磁界Hkのパーマロイ膜厚依存性を示
すグラフの図である。
FIG. 10 is a graph showing the dependency of the anisotropic magnetic field Hk on the thickness of the permalloy film.

【符号の説明】[Explanation of symbols]

1 基板 2 ターゲット 3 成膜面 4 パーマロイ膜 5、7、9 Co膜 6 Cu膜 8 パーマロイ膜 10 反強磁性体層 11 保護層 12 Si(100)面 13 Si基板 14 Si(111)面 15 下部シールド 16 GMR膜 17 上部シールド 18 記録コイル 19 記録コア 20 記録媒体 DESCRIPTION OF SYMBOLS 1 Substrate 2 Target 3 Film-forming surface 4 Permalloy film 5, 7, 9 Co film 6 Cu film 8 Permalloy film 10 Antiferromagnetic layer 11 Protective layer 12 Si (100) surface 13 Si substrate 14 Si (111) surface 15 Lower part Shield 16 GMR film 17 Upper shield 18 Recording coil 19 Recording core 20 Recording medium

───────────────────────────────────────────────────── フロントページの続き Fターム(参考) 5D034 BA02 BA16 DA04 DA07 5E049 AA01 AA07 AA09 AC00 AC05 BA12 BA16 CB02 CC01 DB02 DB04 DB10 DB12 GC01  ──────────────────────────────────────────────────の Continued on the front page F term (reference) 5D034 BA02 BA16 DA04 DA07 5E049 AA01 AA07 AA09 AC00 AC05 BA12 BA16 CB02 CC01 DB02 DB04 DB10 DB12 GC01

Claims (5)

【特許請求の範囲】[Claims] 【請求項1】 スパッタ法を用いて、少なくとも第1の
強磁性層、非磁性層、第2の強磁性層、反強磁性層から
構成される磁気抵抗効果膜を、ターゲット面に対して一
部分が傾いた基板上に形成する磁気抵抗効果膜の製造方
法であって、 少なくとも第1の強磁性層の成膜中に、前記基板に高周
波バイアスを印加することを特徴とする磁気抵抗効果膜
の製造方法。
A magnetoresistive film including at least a first ferromagnetic layer, a nonmagnetic layer, a second ferromagnetic layer, and an antiferromagnetic layer is partially formed on a target surface by sputtering. A method of manufacturing a magnetoresistive film formed on a substrate having a tilt, wherein a high frequency bias is applied to the substrate at least during the formation of the first ferromagnetic layer. Production method.
【請求項2】 前記ターゲットと前記基板のなす角度が
略55°であり、且つ高周波バイアスの電力がターゲッ
トへの投入電力の4%以上であることを特徴とする請求
項1記載の磁気抵抗効果膜の製造方法。
2. The magnetoresistive effect according to claim 1, wherein the angle between the target and the substrate is approximately 55 °, and the power of the high frequency bias is 4% or more of the power applied to the target. Manufacturing method of membrane.
【請求項3】 前記磁気抵抗効果膜を、非晶質基板また
は非晶質膜が成膜された基板上に形成することを特徴と
する請求項1または2記載の磁気抵抗効果膜の製造方
法。
3. The method according to claim 1, wherein the magnetoresistive film is formed on an amorphous substrate or a substrate on which the amorphous film is formed. .
【請求項4】 前記請求項1乃至3記載の製造方法によ
り製造されたことを特徴とする磁気抵抗効果膜。
4. A magnetoresistive film manufactured by the manufacturing method according to claim 1.
【請求項5】 前記請求項4記載の磁気抵抗効果膜を有
する薄膜磁気ヘッド。
5. A thin-film magnetic head having the magnetoresistive film according to claim 4.
JP10306557A 1998-10-28 1998-10-28 Method of manufacturing magnetoresistive film, magnetoresistive film using the same, and thin-film magnetic head Pending JP2000132818A (en)