GB2051640A - Improvements in the cooling of wire rod - Google Patents

Improvements in the cooling of wire rod Download PDF

Info

Publication number
GB2051640A
GB2051640A GB8022240A GB8022240A GB2051640A GB 2051640 A GB2051640 A GB 2051640A GB 8022240 A GB8022240 A GB 8022240A GB 8022240 A GB8022240 A GB 8022240A GB 2051640 A GB2051640 A GB 2051640A
Authority
GB
United Kingdom
Prior art keywords
wire
wire rod
cooling path
cooling
finishing block
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
GB8022240A
Other versions
GB2051640B (en
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kocks Technik GmbH and Co KG
Original Assignee
Kocks Technik GmbH and Co KG
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kocks Technik GmbH and Co KG filed Critical Kocks Technik GmbH and Co KG
Publication of GB2051640A publication Critical patent/GB2051640A/en
Application granted granted Critical
Publication of GB2051640B publication Critical patent/GB2051640B/en
Expired legal-status Critical Current

Abstract

The first portion (3) of a cooling path for cooling hot-rolled wire rod or wire (2) slopes downwardly from a likewise inclined rolling finishing block (1) at an angle ??? of at least 3 DEG so that the wire rod or wire is subject to little or no compressive stress due to the friction between the wire rod or wire and the tube through which the latter passes in order to be subjected to cooling liquid. The wire rod or wire can be placed under tension if the angle of slope alpha is sufficiently large and, in an extreme case the first portion of the cooling path can descend vertically. A loop layer (4) deposits the wire rod or wire in overlapping loops (5) on conveying means (6) where the wire rod or wire is air- cooled. The avoidance or minimizing of compressive stresses in the first cooling section makes the wire rod or wire less prone to buckle. <IMAGE>

Description

SPECIFICATION Improvements in the cooling of wire rod The invention relates to a cooling path for the cooling of hot-rolled wire rod or wire, in which there is provided beyond the last rolling stand of a finishing block a tubular, first portion of the cooling path which subjects the elongated wire to cooling liquid. A loop laying device is generally provided downstream of a cooling path portion of this kind and deposits the wire in overlapping loops onto a conveying means, such as an endless conveyor belt or conveyor rollers, acting as a second portion of the cooling path where the individual loops of wire, overlapping one another, are conveyed away and thereby further cooled by air.
In known cooling paths of this kind, the first portion of the cooling path either extends horizontally between the finishing block and the loop laying device or it slopes upwardly from the delivery end of the finishing block towards the loop laying device.
These known types of construction have the disadvantages that the wire, which is still in a hot state from the rolling operation and is thus of only low strength, is subjected to a relatively high compressive stress of approximately 0.07 to 0.1 kp/mm2. This compressive stress is produced by the friction between the wire and the guide tube of the watercooling path, the friction factor being approximately 0.2 to 0.3, and the length of the first portion of the cooling path generally being approximately 30 metres. There is a considerable risk of buckling as a result of this compressive stress, particularly in the case of high rolling speeds. If the wire rod or wire should buckle, it drags within the guide tubes of the first portion of the cooling path and can even jam in an extreme case.The wire rod or wire is damaged and, if it has jammed, can only be removed from the guide tubes at considerable expense which, of course, involves a long shutdown period.
An object of the invention is to provide a cooling path in which the wire is less prone to buckling even at high run-through speeds.
In accordance with the invention, there is provided a cooling path for the cooling of hotrolled wire rod or wire, in which there is provided beyond the last rolling stand of a finishing block a tubular, first portion of the cooling path which subjects the elongated wire rod or wire to cooling liquid and which descends from the finishing block.
Thus, the compressive stresses in the longitudinal direction of the wire rod or wire can be reduced to a considerable extent and can even be entirely eliminated. Furthermore, it is possible to subject the wire to a corresponding tensile stress which is so small that it cannot break the wire although it maintains the wire in a taut state. Thus, a cooling path of the type in accordance with the invention is particularly operationally reliable and is especially suitable for high rolling speeds.
The run-through axis of the finishing block preferably slopes downwardly and thus has the substantial advantage that the direction of movement of the wire no longer needs to be changed at the location where the wire has already reached a high run-through speed, the change in the direction of movement being effected upstream of the finishing block, that is to say, at a location where the run-through speed is substantially lower and is, for example, approximately 10 to 1 2 metres per second.
In a preferred embodiment of the invention, the first portion of the cooling path slopes downwardly with an angle of slope equal to or greater than 3 degrees. With an angle of slope of, for example, 6 degrees, the compressive stress is only 0.044 kp/mm2 with a friction factor of 0.3 and thus generally lies below the stress which could cause buckling of the wire.
If it is desired to eliminate this slight residual compressive stress, it is possible to increase the angle of slope to an extent that the tangent of the angle of slope is equal to the tangent of the angle of friction or equal to the friction factor. However, with the great length of the first portion of the cooling path, this would mean that there would be a difference in height of approximately 1 2 metres between the finishing block and the loop laying device, which might be precluded by local conditions but which would otherwise be very advantageous.
In an extreme case, the angle of slope of the first portion of the cooling path is approximately 90 degrees. This, of course, presupposes that local conditions permit the resultant great difference in height between the finishing block and the loop laying device.
The finishing block would then have to be disposed at a great height, this being quite conceivable in view of the generally known continuous casting plants which also are of considerable height. In a cooling path of this construction, the wire rod or wire would even be subjected to a tensile stress which would be caused by the weight of the wire rod or wire and which would ensure that the wire rod or wire passes through the first portion of the cooling path in a satisfactory manner without being over-stressed and broken.
A further embodiment of the invention can reside in the fact that the course of the first portion of the cooling path corresponds to the trajectory of the wire. Such a trajectory refers to that curve which would be described by an unbraked, free-falling length of wire rod or wire emerging at rolling speed and which would correspond to the trajectory of a projectile. In this embodiment, neither a tensile stress nor a compressive stress is exerted on the wire rod or wire. The trajectory and thus the construction of the water-cooling path can also be determined, although, of course, this embodiment is only suitable in cases in which the delivery speed of the work material remains constant at the predetermined value.
On the other hand, however, there is the advantage that the compressive stress in the wire rod or wire can be kept at zero when there is a relatively small difference between the height of the finishing block and the height of the loop laying device.
The prior art and the invention are further described, by way of example, with reference to the drawings, in which: Figures 1 and 2 are diagrammatic elevations of two known cooling paths in which the first portion of the cooling path slopes upwardly and extends horizontally respectively; Figures 3 to 6 are similar diagrammatic elevations of three cooling paths in accordance with the invention in which the first portion of the cooling path slopes downwardly; Figure 7 is a more detailed illustration of the embodiment of Fig. 4; and Figure 8 is a graph in which the compressive stress in the wire is plotted against the angle of slope.
Referring to Fig. 1, the wire 2 coming from rolling blocks (not illustrated) enters a finishing block 1 disposed therebeyond. The entry velocity is, for example, approximately 10 to 1 2 metres per second. Owing to the elongation of the wire rod or wire effected during its deformation, the wire rod 2 is delivered from the finishing block 1 at a velocity in excess of 50 metres per second and thus runs at this velocity through a first portion 3 of the cooling path having the length L of approximately 30 metres. At the end of the first portion 3 of the cooling path, the wire 2 enters a loop laying device 4 of known construction by which the wire is deposited in the form of loops 5 overlapping one another, onto a conveying means 6.
In the embodiment of Fig. 1, the first portion of the cooling path slopes upwardly from the finishing block 1 to the loop laying device at an angle a of slope. In this known construction, the finishing block 1 has a horizontal run-through axis, so that the runthrough direction of the wire rod has to be corrected by the angle CL shortly beyond the last rolling stand of the finishing block 1.The friction occuring in the first portion 3 of the cooling path also has to be taken into account, so that the total compressive stress occurring in the wire is calculated as follows: = = y.Ltan(a + 0.10-3 in which a'D represents the compressive stress in kiloponds per square millimetre, y represents the specific gravity of the wire rod, L represents the length of the cooling path, and a represents the angle of slope. + is the angle of friction whose tangent is approximately 0.3, this being equivalent to the friction factor. The angle CL of slope is approximately 6 degrees.
The embodiment of Fig. 2, which is also of known construction, subjects the wire rod to a smaller compressive stress which, however, is still too great, although the angle cu of slope is zero owing to the horizontal arrangement of the first portion of the cooling path. However, a considerable friction factor still causes the compressive stress which is calculated from the following formula: = = y.L.tan +.10-3 Fig. 3 shows an embodiment in accordance with the invention in which the compressive stress in the wire rod is zero. The downward slope of the first portion 3 of the cooling path is clearly shown, as well as the curvature thereof corresponding to the trajectory of the wire 2.The difference in height in the region of the loop forming device is h = 3gut2, g being the acceleration due to gravity, and t being the time in seconds which an elemental length of wire rod under consideration needs to pass through the first portion 3 of the cooling path at the speed at which it is delivered from the last rolling stand. The individual points on the trajectory are calculated by the same formula, the time t being different in each case.
Fig. 4 shows a cooling path in which the first portion 3 of the cooling path slopes relative to the horizontal by an angle cu equal to or greater than 3 degrees. Wnile the slope of the finishing block 1 in the embodiment of Fig. 3 is very smail and is virtually zero, it is clearly shown in the embodiment of Fig. 4 and corresponds to the angle a of slope. This becomes negative, so that the following formula is obtained for calculating the compressive stress in the wire: 5D y.L.tan(-a + 0.10-3 The residual compressive stress to be calculated from this formula is negligible.
This compressive stress aD is zero in the embodiment of Fig. 5, that is to say, when the angle a of slope is equal to the friction angle {.
The angle a of slope is 90 degrees in the further embodiment of the invention shown in Fig. 6, thus resulting in a negative compressive stress, that is to say, a tensile stress az which is calculated by the following formula: = = y.L.10-3 Fig. 7 clearly shows that the wire rod 2 forms a hanging loop 7 upstream of the finishing block 1, thus ensuring that the wire rod 2 enters the finishing block free from tensile and compressive stresses. The reference symbols correspond to those used in the Figures described above. Fig. 7 constitutes an embodiment of the invention which is preferred at the present time, and also shows the second portion of the cooling path with its conveyor element 6, and a bundle-forming station 8 where the cooled loops 5 are collected for form a bundle.
The graph of Fig. 8 shows the compressive stress 4 in the wire 2 plotted against the angle a of slope. The various angles of slope are plotted along the abscissa, whereas the coordinate shows the stress values o'D in kiloponds per square millimetre and in percentages. The curve 9 shown by a solid line applies to the tangent of the friction angle + (that is to say, for a friction factor) of 0.3, whereas the second curve 10 shown by a broken line applies to a friction factor of 0.2.

Claims (6)

1. A cooling path for the cooling of hotrolled wire rod or wire, in which there is provided beyond the last rolling stand of a finishing block a tubular, first portion of the cooling path which subjects the elongated wire rod or wire to cooling liquid and which descends from the finishing block.
2. A cooling path as claimed in claim 1, in which the run-through axis of the finishing block slopes downwardly relative to the horizontal and the first portion of the cooling path slopes downwardly at an angle of at least 3 degrees.
3. A cooling path as claimed in claim 1, in which the first portion of the cooling path corresponds to the trajectory of the wire rod or wire.
4. A cooling path for the cooling of hotrolled wire rod or wire, in which a finishing block is arranged vertically so as to deliver the wire rod or wire downwardly to a first portion of the cooling path which descends substantially vertically.
5. A cooling path as claimed in any preceding claim, in which the second portion of the cooling path is an air cooling path in which the wire rod or wire is conveyed in overlapping loops, a loop laying device being disposed between the first and second cooling path portions.
6. A cooling path for the cooling of hotrolled wire rod or wire, constructed and arranged substantially as herein described with reference to and as illustrated in Figs. 3 to 7 of the drawings.
GB8022240A 1979-07-10 1980-07-08 Cooling of wire rod Expired GB2051640B (en)