CN221985890U - Preparation system of polyester film for composite aluminum foil film - Google Patents

Preparation system of polyester film for composite aluminum foil film Download PDF

Info

Publication number
CN221985890U
CN221985890U CN202323499765.8U CN202323499765U CN221985890U CN 221985890 U CN221985890 U CN 221985890U CN 202323499765 U CN202323499765 U CN 202323499765U CN 221985890 U CN221985890 U CN 221985890U
Authority
CN
China
Prior art keywords
outlet
inlet
aluminum foil
film
stretching
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202323499765.8U
Other languages
Chinese (zh)
Inventor
吴培服
吴迪
刘鸿纬
周振
郑卫
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Shuangxing Color Plastic New Materials Co Ltd
Original Assignee
Jiangsu Shuangxing Color Plastic New Materials Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangsu Shuangxing Color Plastic New Materials Co Ltd filed Critical Jiangsu Shuangxing Color Plastic New Materials Co Ltd
Priority to CN202323499765.8U priority Critical patent/CN221985890U/en
Application granted granted Critical
Publication of CN221985890U publication Critical patent/CN221985890U/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本实用新型公开了一种用于复合铝箔膜的聚酯薄膜的制备系统,至少包括改性处理设备;所述改性处理设备的出口连接高速混合机的入口;所述高速混合机的出口连接排气式双螺杆挤出机的入口;所述排气式双螺杆挤出机的出口连接厚片纵向拉伸设备的入口;所述厚片纵向拉伸设备的出口连接拉伸片横向拉伸机构的入口;所述拉伸片横向拉伸机构的出口连接冷却定型设备的入口;所述冷却定型设备的出口连接分切收卷机构。通过本申请的制备系统制备的聚酯薄膜可以在制备复合铝箔膜的各项处理之后,仍然保持厚薄均匀的状态,不会由于经历复合铝箔膜的制备处理而发生破损和应力卷曲等问题。

The utility model discloses a preparation system of a polyester film for composite aluminum foil film, which at least comprises a modification treatment device; the outlet of the modification treatment device is connected to the inlet of a high-speed mixer; the outlet of the high-speed mixer is connected to the inlet of a venting twin-screw extruder; the outlet of the venting twin-screw extruder is connected to the inlet of a thick sheet longitudinal stretching device; the outlet of the thick sheet longitudinal stretching device is connected to the inlet of a stretching sheet transverse stretching mechanism; the outlet of the stretching sheet transverse stretching mechanism is connected to the inlet of a cooling and shaping device; the outlet of the cooling and shaping device is connected to a slitting and winding mechanism. The polyester film prepared by the preparation system of the present application can still maintain a uniform thickness after various treatments for preparing the composite aluminum foil film, and will not suffer from problems such as breakage and stress curling due to the preparation treatment of the composite aluminum foil film.

Description

Preparation system of polyester film for composite aluminum foil film
Technical Field
The utility model relates to a preparation system of a polyester film for a composite aluminum foil film.
Background
In lithium ion batteries, aluminum foil is commonly used as the positive current collector, and copper foil is commonly used as the negative current collector. In order to increase the energy density of the battery, composite current collectors using a composite of a plastic film and a metal layer, such as a composite aluminum current collector used as a positive electrode and a composite copper current collector used as a negative electrode, have appeared. The metal layer in the composite current collector is bonded to the plastic film by a metal foil, and is formed on the plastic film by an evaporation or sputtering process. The metal foil has excellent conductivity but a thicker thickness; the metal layer formed by sputtering and vapor plating has thinner thickness, poorer conductivity, repeated film plating is needed for many times, the process requirement is high, the repeated film plating of the plastic film is easy to wrinkle, the yield is lower, and the cost is high.
For example, CN 114695900B discloses a composite current collector, including first aluminium foil layer, PET layer and the second aluminium foil layer of range upon range of setting in proper order, first aluminium foil layer and second aluminium foil layer all with PET layer fixed connection, the up end on first aluminium foil layer is provided with a plurality of first recesses, the lower terminal surface on second aluminium foil layer is provided with a plurality of second recesses. This current is in order to obtain the recess, has adopted thicker aluminium foil structure.
Then, the aluminum foil and copper foil used as current collectors are mainly used for conduction and do not participate in the active reaction. One of the means of increasing the energy density of the battery at this stage is thus to reduce the mass ratio of the current collector: on the one hand, a composite metal foil film with smaller density is adopted, and on the other hand, the thickness of the metal layer is reduced. The use of thicker aluminum foil is not desirable at this stage.
Disclosure of Invention
The technical problem to be solved by the application is to provide a preparation system of a polyester film for a composite aluminum foil film, so as to reduce or avoid the problems.
In order to solve the technical problems, the application provides a preparation system of a polyester film for a composite aluminum foil film, which at least comprises modification treatment equipment for nano montmorillonite; the outlet of the modification treatment equipment is connected with the inlet of a high-speed mixer for high-speed mixing of polyisobutylene succinimide, tetrabutyl titanate, 1, 4-dimethoxy benzene, cyanoacrylate, nano modified montmorillonite particles and PET slices; the outlet of the high-speed mixer is connected with the inlet of the exhaust double-screw extruder; the outlet of the exhaust double-screw extruder is connected with the inlet of the thick sheet longitudinal stretching equipment; the outlet of the thick sheet longitudinal stretching device is connected with the inlet of the stretching sheet transverse stretching mechanism; an outlet of the stretching sheet transverse stretching mechanism is connected with an inlet of the cooling shaping equipment; and an outlet of the cooling shaping equipment is connected with the slitting and winding mechanism.
Preferably, the modification treatment apparatus includes: the dispersing tank is used for dispersing nano montmorillonite into a polyvinyl alcohol aqueous solution, an outlet of the dispersing tank is connected with a first inlet of a freeze-drying spraying device, the freeze-drying spraying device is connected with an inlet of a cleaning tank through a pipeline, an outlet of the cleaning tank is connected with a second inlet of the freeze-drying spraying device through a pipeline, and the freeze-drying spraying device is connected with the high-speed mixer through a modified outlet pipeline.
The polyester film prepared by the preparation system can still keep a state of uniform thickness after various treatments of preparing the composite aluminum foil film, and the problems of breakage, stress curling and the like caused by the preparation treatment of the composite aluminum foil film are avoided.
Drawings
The following drawings are only for purposes of illustration and explanation of the present application and are not intended to limit the scope of the application.
Fig. 1 shows a cross-sectional view of a composite aluminum foil film according to an embodiment of the present application.
Fig. 2 is a schematic view showing the construction of a system for preparing a polyester film for a composite aluminum foil film according to an embodiment of the present application.
Detailed Description
For a clearer understanding of technical features, objects, and effects of the present application, a specific embodiment of the present application will be described with reference to the accompanying drawings. Wherein like parts are designated by like reference numerals.
The existing lithium battery generally adopts a metal aluminum foil obtained by rolling metal aluminum as a positive current collector, and the thickness of the adopted metal aluminum foil is difficult to reduce due to the strength limitation of the material, otherwise, the metal aluminum foil is easy to tear in the operation process. Even if the metal aluminum foil and the plastic film are compounded together, the compounding operation cannot be performed by using the metal aluminum foil which is too thin.
In view of this, the present application proposes a composite aluminum foil film composed of a base material layer 1 and metal aluminum foils 2 adhered to both sides of the base material layer 1, as shown in fig. 1. The substrate layer 1 can be made of plastic films made of polyolefin, polyester and other materials. In a preferred embodiment, the substrate layer 1 is preferably made of a polyester film. The metal aluminum foil 2 can be adhered to both sides of the substrate layer 1 through an adhesive.
Further, the metal aluminum foil 2 in the composite aluminum foil film of the present application may be composed of a metal aluminum foil of a first thickness of 5-15 μm and a metal aluminum foil of a second thickness of 3-8 μm laminated and stretched on both sides of the base material layer 1. That is, the metal aluminum foil 2 of the present application initially has a first thickness, and is rolled and stretched by being attached to both sides of the base material layer 1, and then becomes a final second thickness. Because the material strength of the metal aluminum is not good, the metal aluminum foil with the second thickness of 3-8 mu m is directly adopted, the price is high, the bonding and other composite operations are difficult to carry out, therefore, the application adopts the metal aluminum foil with the first thickness of 5-15 mu m as the initial raw material, the metal aluminum foil is bonded and compounded with the base material layer 1, then the rolling and stretching operation is carried out to change the metal aluminum foil into the second thickness, and then the composite operation is not needed, so that the thinner metal aluminum foil can be obtained, and the conductivity and the strength can be ensured.
For example, the metallic aluminum foil 2 used is rolled from metallic aluminum having an aluminum content exceeding 98%, and a commercially available finished metallic aluminum foil product having a thickness of 5 to 15 μm can be selected as the initial raw material of the first thickness.
Further, as shown in the figure, a layer of rolling protection film 3 is further attached to the outer side of the metal aluminum foil 2, so as to protect the surface of the metal aluminum foil 2 from being scratched and broken in the rolling and stretching process. The rolling protective film 3 can also be prepared from plastic films made of polyolefin, polyester, nylon and other materials. In a preferred embodiment, the laminate protective film 3 is preferably made of a nylon film excellent in strength and self-lubricating properties, preferably a nylon film having a thickness of 8 to 10 μm.
When the composite aluminum foil film is prepared, the two sides of the substrate layer 1 with the initial thickness of 10-20 mu m can be coated with the adhesive, and then the metal aluminum foil 2 with the first thickness is adhered on the surface of the substrate layer 1. After that, lubricating oil such as engine oil or silicone grease may be coated on the outer side of the metal aluminum foil 2, and then a rolling protective film 3 made of, for example, nylon with a thickness of 8-10 μm is attached to the surface of the oiled metal aluminum foil 2. By coating the lubricant, the adhesive force of the rolling protective film 3 on the metal aluminum foil 2 can be increased, and meanwhile, the friction force can be reduced in the subsequent rolling expansion process, so that the film layer is prevented from being broken.
Then, the film layer to which the laminate protective film 3 is attached is placed between at least a pair of laminating rollers, and the metal aluminum foil 2 is laminated from the first thickness to a second thickness of 3-8 μm by the pressure of the laminating rollers. The film layer structure is easy to damage by thinning the film layer in a pure hard extrusion mode, so that the rolling protection film 3 contacted with the rolling roller is made of nylon, the slidability can be improved, the extrusion is avoided, and meanwhile, the friction force between the film layer and the rolling roller during rolling can be further reduced by auxiliary coating of lubricating oil. After the rolling and stretching, the thickness of the base material layer 1 is changed from 10 to 20 μm to about 6 to 12 μm.
In addition, can heat the rete before the rete rolls through the roll that rolls to increase plastic film's ductility, improve the efficiency of rolling the attenuation, the resilience volume of plastic film after the heating can reduce simultaneously, is favorable to keeping the rete thickness after stretching. In a preferred embodiment, the film layer may be heated by infrared heating, preferably at a temperature of 150-170 ℃.
In addition, the two sides of the film layer can be stretched outwards while the film layer is rolled by the rolling roller. That is, the film layer is longitudinally stretched by the laminating roller while being transversely stretched by sandwiching both sides in the width direction by the sandwiching means, so as to accelerate the thinning speed of the material. Because the stretching problem of the metal aluminum foil is involved, the whole film layer is required to be clamped during clamping and stretching, the transverse stretching speed is controlled, and the problem of inconsistent stretching proportion between the film layers is avoided.
In addition, after the film layer is rolled and stretched, in order to avoid the stress to rebound the film layer, the film layer can be further subjected to thermal annealing so as to eliminate the stress in the film layer. The annealing temperature is preferably 130-150 ℃ and the annealing time is 5-15 minutes.
Finally, removing the rolling protection film 3 of the annealed film layer, removing lubricating oil on the outer surface of the metal aluminum foil 2 by using a cleaning agent, and then washing with clear water, drying, trimming and rolling to obtain the composite aluminum foil film.
By describing the structure and the preparation process of the composite aluminum foil film, the application further provides a polyester film suitable for the composite aluminum foil film, and the polyester film is used as the substrate layer 1 of the composite aluminum foil film. The substrate layer 1 prepared by the polyester film of the application has excellent mechanical properties, can be subjected to the heating, rolling stretching and annealing treatment of the composite aluminum foil film of the application, and maintains a state of uniform thickness after the treatment, and can not cause the problems of breakage, stress curling and the like due to the preparation treatment of the composite aluminum foil film.
Specifically, the application provides a polyester film for a composite aluminum foil film, which is used as a base material layer 1 of the composite aluminum foil film, wherein metal aluminum foils 2 are bonded to two sides of the base material layer of the composite aluminum foil film, and the metal aluminum foils 2 can be formed by rolling and stretching metal aluminum foils with a first thickness of 5-15 mu m and a second thickness of 3-8 mu m on two sides of the base material layer. The polyester film is prepared from the following components in parts by weight: 10-20 parts of polyisobutylene succinimide, 1-3 parts of tetrabutyl titanate, 3-5 parts of 1, 4-dimethoxy benzene, 5-10 parts of cyanoacrylate, 2-4 parts of nano modified montmorillonite particles and 1000-2000 parts of PET slices. In one embodiment of the present application, 10 to 20 parts by weight of polyisobutylene succinimide, 1 to 3 parts by weight of tetrabutyl titanate, 3 to 5 parts by weight of 1, 4-dimethoxybenzene, 5 to 10 parts by weight of cyanoacrylate, 2 to 4 parts by weight of nano modified montmorillonite particles, and 1000 to 2000 parts by weight of PET chips may be added into a high speed mixer at normal temperature to be pre-dispersed and mixed at a rotational speed of 1500 to 2000rpm for 30 to 60 minutes to form a mixture. And then the mixture enters an exhaust double-screw extruder, and the temperature of the double-screw extruder is adjusted to 270-280 ℃. After the materials are melted in an extruder, the materials are filtered and extruded into thick sheets. The thickness and profile of the slab can be adjusted by the extrusion amount of the extruder, the rotation speed of the casting roll and the opening degree of the die head. Preheating the thick sheet at 50-90 ℃, entering an infrared heating zone at 300-500 ℃, and longitudinally stretching at a linear speed of 40-150 m/min to obtain a stretched sheet, wherein the longitudinal stretching multiplying power is 4.0. Preheating the stretching sheet at 90-120 ℃, and transversely stretching at 100-160 ℃ with a transverse stretching multiplying power of 3.8. And then shaping at 160-240 ℃, and cooling at 100-50 ℃ to obtain the polyester film. The prepared polyester film can be cut and rolled for standby. Wherein, in order to facilitate the uniform dispersion of the nano montmorillonite in the organic component of the polyester film, the nano montmorillonite needs to be subjected to surface modification treatment. The method comprises the following specific steps: adding 10-20 parts by weight of nano montmorillonite into 100-200 parts by weight of polyvinyl alcohol water solution, and continuously stirring for 60-120 minutes to fully disperse; then freeze-drying and spraying the dispersion mixture to obtain a solid particle mixture subjected to surface modification treatment; adding the obtained solid particle mixture into clear water, washing and filtering for multiple times to obtain a dispersion liquid which does not contain soluble matters and has the solid content of 20-40wt%, freeze-drying and spraying the dispersion liquid again, and sieving to select particles with the particle size of 10-20nm to obtain the nano modified montmorillonite particles. Wherein the content of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 10-15 wt%.
Correspondingly, the application also provides a preparation system of the polyester film for the composite aluminum foil film, as shown in fig. 2. In the specific embodiment shown in fig. 2, the preparation system of the present application comprises at least a modification treatment apparatus 300 for nano montmorillonite. The outlet of the modification treatment apparatus 300 is connected to the inlet of a high-speed mixer 101 for high-speed mixing of polyisobutylene succinimide, tetrabutyl titanate, 1, 4-dimethoxy benzene, cyanoacrylate, nano modified montmorillonite particles, and PET chips.
The outlet of the high-speed mixer 101 is connected with the inlet of the exhaust double-screw extruder 102; the outlet of the exhaust double-screw extruder 102 is connected with the inlet of the thick sheet longitudinal stretching device 103; the outlet of the thick sheet longitudinal stretching device 103 is connected with the inlet of the stretching sheet transverse stretching mechanism 104; the outlet of the stretching sheet transverse stretching mechanism 104 is connected with the inlet of the cooling shaping equipment 105; and an outlet of the cooling shaping equipment 105 is connected with a slitting and winding mechanism 106.
In another embodiment of the present application, as shown in fig. 2, the modification treatment apparatus 300 includes: a dispersion tank 301 for dispersing nano montmorillonite into a polyvinyl alcohol aqueous solution, an outlet of the dispersion tank 301 is connected with a first inlet 3021 of a freeze-drying spraying apparatus 302, the freeze-drying spraying apparatus 302 is connected with an inlet of a cleaning tank 303 through a pipeline, an outlet of the cleaning tank 303 is connected with a second inlet 3022 of the freeze-drying spraying apparatus 302 through a pipeline, and the freeze-drying spraying apparatus 302 is connected with the high-speed mixer 101 through a modified outlet pipeline 304.
Examples 1 to 5
Polyester films for a base material layer of a composite aluminum foil film were prepared respectively in the weight part ratio of the raw materials in the following table.
Example 1 Example 2 Example 3 Example 4 Example 5
Polyisobutylene succinimides 10 12 15 18 20
Tetrabutyl titanate 1.0 1.5 2.0 2.5 3.0
1, 4-Dimethoxybenzene 3.0 3.5 4.0 4.5 5.0
Cyanoacrylate esters 5.0 6.0 7.5 9.0 10.0
Nano modified montmorillonite particles 2.0 2.5 3.0 3.5 4.0
PET 1000 1200 1500 1800 2000
Thickness of polyester film μm 10 12 15 18 20
Comparative examples 6 to 10
Polyester films for comparison were prepared in the same manner as in the above examples in the proportions by weight of the raw materials shown in the following table.
Comparative example 6 Comparative example 7 Comparative example 8 Comparative example 9 Comparative example 10
Polyisobutylene succinimides 0 12 15 20 22
Tetrabutyl titanate 3.0 0 3.5 4.5 4.0
1, 4-Dimethoxybenzene 5.0 4.0 0 6.5 6.0
Cyanoacrylate esters 10.0 6.0 9.0 0 10.0
Nano modified montmorillonite particles 4.0 3.5 5.0 4.5 0
PET 1000 1200 1500 1800 2000
Thickness of polyester film μm 10 12 15 18 20
The performance parameters of the polyester films obtained by the respective test preparation were compared with films of 15 μm thickness prepared from pure PET without any components added. The properties of the finally produced composite aluminum foil films were examined by subjecting examples 1 to 5, comparative examples 6 to 10, and comparative pure PET films as the base material layers of the present application to treatments such as adhesion of metal aluminum foil, rolling and stretching, respectively. Tests show that the polyester films of examples 1-5 can be kept in a state of uniform thickness after various treatments for preparing the composite aluminum foil film, and defects such as breakage, stress curling and the like are not found due to the treatment for preparing the composite aluminum foil film. While comparative examples 6-10 and the virgin PET films failed to undergo the preparation process, various degrees of breakage and curling were found. In conclusion, the polyester film prepared by the preparation system can still keep a state of uniform thickness after various treatments for preparing the composite aluminum foil film, and the problems of breakage, stress curling and the like caused by the treatment for preparing the composite aluminum foil film are avoided.
It should be understood by those skilled in the art that while the present application has been described in terms of several embodiments, not every embodiment contains only one independent technical solution. The description is given for clearness of understanding only, and those skilled in the art will understand the description as a whole and will recognize that the technical solutions described in the various embodiments may be combined with one another to understand the scope of the present application.
The foregoing is illustrative of the present application and is not to be construed as limiting the scope of the application. Any equivalent alterations, modifications and combinations thereof will be effected by those skilled in the art without departing from the spirit and principles of this application, and it is intended to be within the scope of the application.

Claims (2)

1. A preparation system for polyester film of composite aluminum foil film, characterized in that it comprises at least a modification treatment device (300) for nano montmorillonite; the outlet of the modification treatment equipment (300) is connected with the inlet of a high-speed mixer (101) for mixing polyisobutylene succinimide, tetrabutyl titanate, 1, 4-dimethoxy benzene, cyanoacrylate, nano modified montmorillonite particles and PET slices at high speed; the outlet of the high-speed mixer (101) is connected with the inlet of the exhaust double-screw extruder (102); the outlet of the exhaust double-screw extruder (102) is connected with the inlet of the thick sheet longitudinal stretching equipment (103); the outlet of the thick sheet longitudinal stretching device (103) is connected with the inlet of the stretching sheet transverse stretching mechanism (104); the outlet of the stretching sheet transverse stretching mechanism (104) is connected with the inlet of the cooling shaping equipment (105); and an outlet of the cooling shaping equipment (105) is connected with a slitting and winding mechanism (106).
2. The production system according to claim 1, wherein the modification treatment apparatus (300) includes: a dispersion tank (301) for dispersing nano montmorillonite into polyvinyl alcohol aqueous solution, the outlet of dispersion tank (301) is connected with a first inlet (3021) of a freeze-drying spraying apparatus (302), the freeze-drying spraying apparatus (302) is connected with the inlet of a cleaning tank (303) through a pipeline, the outlet of the cleaning tank (303) is connected with a second inlet (3022) of the freeze-drying spraying apparatus (302) through a pipeline, and the freeze-drying spraying apparatus (302) is connected with the high-speed mixer (101) through a modified outlet pipeline (304).
CN202323499765.8U 2023-12-20 2023-12-20 Preparation system of polyester film for composite aluminum foil film Active CN221985890U (en)