CN1699666A - Teased long staple adhesive lining cloth and method for manufacturing same - Google Patents

Teased long staple adhesive lining cloth and method for manufacturing same Download PDF

Info

Publication number
CN1699666A
CN1699666A CN 200510040109 CN200510040109A CN1699666A CN 1699666 A CN1699666 A CN 1699666A CN 200510040109 CN200510040109 CN 200510040109 CN 200510040109 A CN200510040109 A CN 200510040109A CN 1699666 A CN1699666 A CN 1699666A
Authority
CN
China
Prior art keywords
fabric
grams per
temperature
per liter
teased
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 200510040109
Other languages
Chinese (zh)
Inventor
黄立刚
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Boseki Co Ltd
Original Assignee
Nitto Boseki Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Boseki Co Ltd filed Critical Nitto Boseki Co Ltd
Priority to CN 200510040109 priority Critical patent/CN1699666A/en
Publication of CN1699666A publication Critical patent/CN1699666A/en
Pending legal-status Critical Current

Abstract

The present invention relates to a kind of manufacturing method for binding lapping cloth of nappy long fiber. Its long fiber radical cloth goes through refining, boiling, bleaching, dyeing, and then dressing and processing. During the latter process, a specific nappy dressing and processing technology is added, so as to achieve the requirements of good touch and shrinkage as expected. Finally, one or double layers of point-like binding agent is pasted on one side of the radical cloth. The invention has the following characters: the lapping cloth is soft, thick and low in water penetration at its reverse side.

Description

Teased long staple adhesive lining cloth and manufacture method thereof
Technical field
The present invention relates to field of textiles, specifically be a kind of Teased long staple adhesive lining cloth and manufacture method thereof.The advantage that this lining cloth has condensed long and short two kinds of fibers: good elasticity, flexibility, solid sense, be applicable on the lining that needs special effect, be specially adapted to thick and heavy lining, not only can increase its warm soft effect, and its extremely low reverse side infiltration can not influence the characteristic of lining.
Background technology
China's binding lining use and development is started late, approximately after the open gateway of a country of late nineteen seventies, introduced advanced technology, equipment from external, just beginning has had bigger development.In from then on 20 years, the binding lining manufacturing industry develops rapidly, and the use of binding lining on clothes is quite general.And along with China's entry into the WTO, improving constantly of development and national economy and living standards of the people, requirement to clothes, fashionable dress is also higher, corresponding with it, the various newfashioned fashionable dresses of garment sector, lining also make rapid progress, and therefore the class of binding lining, technical merit etc. are also had higher requirement.
Summary of the invention
The objective of the invention is to seek a kind of Teased long staple adhesive lining cloth and manufacture method thereof, this lining cloth has good stable and super soft abundant effect.
According to design provided by the present invention, have on the surface of fabric and to utilize the physical mechanical active force that the weft yarn of fabric is ticked to break one deck fine hair that the back forms, and the point-like resin.
The manufacture method of Teased long staple adhesive lining cloth is characterized in that,
Refining: refining in the High Temperature High Pressure liquid-flow dyeing machine, after being warming up to 75~85 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the fluid cylinder that coexists, in this process, add entry to required amount and auxiliary agent, be warming up to 90~100 ℃ of concise temperature then, after concise 5~20 minutes, venting refining liquid takes out behind the adding cold water washing;
Arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, after making above-mentioned refined fabric soak into dressing liquid, enter again in the mechanical baking oven of arrangement, under 90 ℃~210 ℃ temperature, make the fabric drying typing, 25~40 meters/minute of the speed of a motor vehicle;
The fluffing arrangement: put into the fluffing arrangement mechanically through the fabric behind the arrangement mechanical finishing, utilize the physical mechanical active force that the weft yarn of fabric is ticked and break, form one deck fine hair at fabric face, its speed of a motor vehicle 10-25 rice/minute;
Bonding: make fabric after the above-mentioned fluffing arrangement through coating machine, at the bonding point-like resin of fabric face, stentering forming in stenter again, 130~180 ℃ of tentering temperature, its process velocity is: 20~45 meters/minute.
The composition of the auxiliary agent in the described concise liquid is softener 0.1~0.5 grams per liter, surfactant 0.1~0.5 grams per liter, NaOH 2~10 grams per liters, desizing agent 0.3~0.6 grams per liter in metal ion chelation agent 0.1~0.5 grams per liter, the bath, Yu Weishui.
The composition of the auxiliary agent in the described dressing liquid is softener 2~6 grams per liters, antistatic agent 0.1~1.5 grams per liter, bleeding agent 0.1~0.3 grams per liter, waterproofing agent 0.5~3.0 grams per liter, Yu Weishui.
In when arrangement fluffing, can utilize bearded needle on the fluffing collator that the weft yarn of fabric is ticked and break, carry out at normal temperatures.
Engraved roll, a roller, No. two rollers and No. three rollers are arranged in coating machine, and its temperature is an engraved roll: 30~40 ℃, No. one roller~No. three roller is 150~210 ℃.
After refining, in the high temperature liquid-flow dyeing machine, add the dye liquor of entry and auxiliary agent preparation again, under 100~150 ℃ temperature, dyeed through 20~50 minutes.
The addition of auxiliary agent is DISPERSE DYES 5~20 grams per liters in the dyeing, softener 0.5~1.5 grams per liter in the bath, dispersant 0.3~1 grams per liter, formic acid 0.1~0.3 grams per liter, Yu Weishui.
Soap after dyeing, soaped 10~30 minutes in the liquid of soaping of water and soaping agent preparation, temperature is 70~100 ℃; And then washing: wash in clear water, 10~20 minutes time, temperature is a normal temperature.
Described resin is polyamide-based, polyethylene, copolyamide class, polyester, polyvinyl alcohol.
When bonding, the mode that can utilize the net tube to shift is coated on prime cement on the fabric base cloth surface with point-like, the spreading powdered resin equably again, absorb unnecessary resin then, the place that prime cement is arranged on the base cloth is stained with or keeps resin, carry out Infrared Heating, temperature again: 220~270 ℃, make prime cement dry and be bonded on the fabric base cloth surface, enter drying room then and make fabric typing, 100~140 ℃ of drying room temperature, 25~45 meters/minute of process velocities.Utilize this mode can produce the binding lining that scribbles double-layer resin.
Described prime cement can be the copolymer of POLYPROPYLENE GLYCOL and polypropylene alcohol ester and the colloid that water is formed.
When producing the binding lining of single-layer resin, bonding process is, above being covered with the bond roll of pit, the hopper of adorning powdered resin is arranged, the temperature of bond roll is 150~180 ℃, and bond roll rotates, and powdered resin just falls in the pit of bond roll, exist side by side molten condition, make fabric paste bond roll and pass through, the resin in the pit just is adhered to fabric face, forms the resin of point-like; Whether after being coated with the point-like resin, seeing needs decision that resin is flattened on fabric face.
Described fabric is made through weaving by the stagnant long fiber material of full pin.
Binding lining of the present invention is mainly used in fashionable dress, costume design, on the basis of performance that does not influence lining itself and outward appearance visual effect, gives fabric soft more plentiful characteristic.Simultaneously because this lining cloth has good stable and shrinkage, in time under higher temperature as 140 ℃, when lining and lining cloth hot calendering bonding, can not cause outward appearance deformation, variations such as look change.So when the lining of this kind feel and visual effect is wanted in design processing, select for use this lining cloth can receive fantacy less than effect, and its ultralow reverse side penetrating power has improved the moral character of dress ornament to a great extent, has improved productive value greatly.
Binding lining of the present invention is to carry out one specific fluffing arrangement processing again after being processed through refining, dyeing, arrangement by base cloth: the crochet hook on the machinery drum is put in the utilization fluffing in order, when fabric process cylinder, bearded needle moves up and down, under the effect of eave tile by mechanical force, regularly the fabric weft yarn is ticked and broken, form fluffing.The length of fluffing can be regulated according to the size of mechanicals efforts.And the product after the fluffing had both kept original stability, had added more flexibility again.Carry out the resin finishing operation through coating machine after finishing.
Described base cloth is made by full terylene or nylon long fiber material.Mainly be to spin cloth because as do base cloth with nonwoven fabric, after the washing, anti-ly draw, wash each side such as intensity obvious decline is all arranged, concrete specification is according to various parameters decisions such as the feel of product requirement, bonding forces.Which kind of material binding lining selects for use is that base cloth will be looked it and produces to be used for which kind of lining after the finished product, and the design style of clothes and feel require and decide.Close or the principle of identity according to shrinkage factor: be used for cotton fabric and then select the cotton base cloth for use, by that analogy: the polyester-cotton blend lining is corresponding to the polyester-cotton blend base cloth, and full terylene, full nylon facing material are corresponding to full terylene, full nylon long fiber base cloth.
In the process of using binding lining processing fashionable dress/clothes of the present invention, in advance that clothes/fashionable dress design is selected lining passes through hot calendering bonding together with the selected binding lining that can cooperate with this lining (method as mentioned above) under the temperature heating on 100 ℃~140 ℃ of right sides, together carry out cutting then, be sewn into ready-made clothes.
Base cloth difference then processing method is also different, because the material different performance is different, the process route of design has certainly than big-difference.For long fiber, the effect of each treatment process is as follows:
1, refining:
Form by long fiber terylene or nylon textile, thus owing to do not contain cotton and do not have field trashes such as glue, cotton wax, seed coat, in refining process, only need with the second time field trash remove and get final product.Because long stapled particularity must be carried out boiling-off with long stapled base cloth under lax state, when removing impurity, also to add NaOH.H simultaneously 2O 2The corrosion of long stapled fiber is attenuated so that removes gloss and acquisition is easily dyed, characteristic such as soft, flexible Deng medicine.
2, dyeing: dyestuff is adhered to or be bonded to fiber or enter fibrous inside, make fabric obtain attractive in appearance, even, firm color, and with require sample identical.
In order to keep long fiber fabric better elastic, long stapled dyeing continuation is adopted high temperature, high pressure liquid stream dyeing machine or high temperature, high pressure liquid stream jet dyeing machine DISPERSE DYES (terylene), ACID DYES (nylon) or dispersion/directly (composite core) dyeing down with lax state.
3, arrangement: utilize the technology of the method for physics or chemistry to the processing of base cloth enforcement sense organ.
Chemical method: make after refining, the dyeing the lax fully and base cloth tentering that shrinks to certain fabric width, the typing of heating then.In this process,, make base cloth after arrangement processing, not only have smooth outward appearance, and had certain elasticity, anti-static ability by adding softener, antistatic additive infiltration base cloth, oven dry, and the feel that has design to need.
Physical method: utilize mechanicals efforts the out-of-flatness that becomes of smooth fabric face, thereby reach the effect of anticipation.
4, bonding:
Double-deck when bonding, the way that available hot melt shifts makes resin (PA) be point-like and scatters equably and be bonded on the base cloth 10, and the slurry that applies one deck spot distribution on base cloth is spilt one deck then thereon and had dystectic copolyamide resinoid oven dry and form.1 is baking oven among the figure, and 2 is retracting device, and 3 is air pump, and 4 is dusting device, and 5 is scraper plate, and 6 are the net tube, and 7 is resin slurry, and 8 is cylinder, and 9 is device of excitation, and 10 is base cloth, and 11 is the point-like slurry, and 12 is powdered resin, and 13 for being bonded at the resin on the point-like slurry.Base cloth is through cylinder and after netting between tube, slurry comes out from the mesh of net tube, becomes point-like to be bonded on the base cloth, and base cloth continues reach, at the dusting device place, sprinkled one deck powdered resin, then, after the vibrating device vibration, make powdered resin be sprinkling upon on the base cloth equably, behind air pump and retracting device, the unnecessary powdered resin between the point-like slurry is absorbed again, made powdered resin become point-like to be uniformly distributed in the base cloth surface.
The bonding concrete grammar of individual layer is: the A roller is inner heating, is uniform-distribution with the upper glue roller of pit on the surface.When the A roller rotates, the polyamide-based resin of the powdery in the hopper 14 falls in the pit and melted by heating, adheres to cooling on the grey cloth 10, looks to have or not arts demand again, whether decision utilizes pressure roller D1, D2 to flatten on grey cloth 10 resin 15 of powder point-like, comes out to be finished product.
No matter which kind of lining, which kind of fashionable dress, the soft comfortable a kind of fashion idea that has obviously become people's pursuit.Especially for heavy fabric, because the characteristics of itself, determined it to lack soft plentiful effect, and the appearance of Teased long staple adhesive lining cloth is exactly in order better to change and remedy this weakness of heavily fabric: because the existence of its fabric face fine hair, mutual active force between stiff sense when having weakened fiber and fibre frictoin to a great extent and the fabric, make it soft plentiful comfortable, thereby effectively improved the pliability of heavily fabric, so it have very big development space and potentiality.
Characteristics of the present invention are: on the basis of general long fiber lining cloth, increased soft plentiful characteristic, reduced the reverse side penetrating power simultaneously, thereby given lining better effect, and various reference data has been at all unaffected.
The fluffing arrangement processing of general staple fibre is very general, because the change of texture makes fabric lose resilience, and long fiber is because the characteristics of fibre structure, easy of colluding the texture that silk destroys fabric in the process of fluffing, cause waste product, the invention solves this class problem, when keeping the fluffing advantage, also kept the original characteristics of some long fibers.
The characteristics of processing technology: after general arrangement processing, increased fluffing arrangement processing together.
Description of drawings
Fig. 1 is a double-layer resin adhesive article schematic diagram.
Fig. 2 shifts legend for hot melt.
The specific embodiment
Embodiment one
Raw material: T32432 terylene
1, concise: the concise liquid that is mixed with by water and auxiliary agent that in the liquid bath of concise machinery, adds required amount, the composition of auxiliary agent is softener 0.1 grams per liter, surfactant 0.1 grams per liter, NaOH 3 grams per liters, desizing agent 0.5 grams per liter in metal ion chelation agent 0.1 grams per liter, the bath, Yu Weishui, after being warming up to 75 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the liquid bath that coexists, be warming up to 95 ℃ of concise temperature then, after concise 5 minutes, venting refining liquid takes out behind the adding cold water washing;
2, arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, the composition of auxiliary agent is softener 2 grams per liters, antistatic agent 0.5 grams per liter, waterproofing agent 0.5 grams per liter, bleeding agent 0.2. grams per liter, Yu Weishui, after making above-mentioned refined fabric padding finishing liquid, enter again in the mechanical baking oven of arrangement, under 90 ℃ temperature, make the fabric drying typing, 25 meters/minute of the speed of a motor vehicle;
3, fluffing arrangement:, utilize the physical mechanical active force to collude silk fluffing, 10 meters/minute of the speed of a motor vehicle by the machinery that fluffs;
4, bonding: the mode of utilizing the net tube to shift, prime cement is coated on the base cloth surface with point-like equably, the spreading powdered resin is absorbed unnecessary resin then again, the place that prime cement is arranged on the base cloth is stained with or keeps resin, carry out Infrared Heating again, temperature: 180 ℃, make prime cement dry and be bonded on the base cloth surface, enter the drying room typing then, 100 ℃ of drying room temperature, 25 meters/minute of process velocities;
Make above-mentioned fabric process coating machine through arrangement, be coated with the resin bed of point-like on fabric, engraved roll, a roller, No. two rollers and No. three rollers are arranged in the machine, its temperature is an engraved roll: 30 ℃, No. one roller~No. three roller is 150 ℃, and temperature of oven is 100 ℃.
Embodiment two
Raw material: T32432 terylene
1, concise: the concise liquid that is mixed with by water and auxiliary agent that in the liquid bath of concise machinery, adds required amount, the composition of auxiliary agent is softener 0.3 grams per liter, surfactant 0.3 grams per liter, NaOH 4 grams per liters, desizing agent 0.5 grams per liter in metal ion chelation agent 0.3 grams per liter, the bath, Yu Weishui, after being warming up to 80 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the liquid bath that coexists, be warming up to 90 ℃ of concise temperature then, after concise 15 minutes, venting refining liquid takes out behind the adding cold water washing.
2, arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, the composition of auxiliary agent is softener 4 grams per liters, antistatic agent 0.3 grams per liter, waterproofing agent 1.5 grams per liters, Yu Weishui, after making above-mentioned refined fabric padding finishing liquid, enter again in the mechanical baking oven of arrangement, under 200 ℃ temperature, make the fabric drying typing, 40 meters/minute of the speed of a motor vehicle;
3, fluffing arrangement:, utilize the physical mechanical active force to collude silk fluffing, 20 meters/minute of the speed of a motor vehicle by the machinery that fluffs;
4, bonding: as to make above-mentioned fabric process coating machine through arrangement, be coated with the resinoid of point-like on fabric, engraved roll, a roller, No. two rollers and No. three rollers are arranged in coating machine, its temperature is an engraved roll: 40 ℃, No. one roller~No. three roller is 210 ℃, and temperature of oven is 130 ℃.
Embodiment three
Raw material: T32432 terylene
1, concise: the concise liquid that is mixed with by water and auxiliary agent that in the liquid bath of concise machinery, adds required amount, the composition of auxiliary agent is softener 0.2 grams per liter, surfactant 0.2 grams per liter, NaOH 3 grams per liters, desizing agent 0.4 grams per liter in metal ion chelation agent 0.2 grams per liter, the bath, Yu Weishui, after being warming up to 85 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the liquid bath that coexists, be warming up to 95 ℃ of concise temperature then, after concise 10 minutes, venting refining liquid takes out behind the adding cold water washing.
2, arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, the composition of auxiliary agent is softener 3 grams per liters, antistatic agent 0.5 grams per liter, waterproofing agent 1.0 grams per liters, Yu Weishui, after making above-mentioned refined fabric padding finishing liquid, enter again in the mechanical baking oven of arrangement, under 150 ℃ temperature, make the fabric drying typing, 30 meters/minute of the speed of a motor vehicle;
3, fluffing arrangement:, utilize the physical mechanical active force to collude silk fluffing, 20 meters/minute of the speed of a motor vehicle by the machinery that fluffs;
4, bonding: as to make above-mentioned fabric process coating machine through arrangement, be coated with the resin of point-like on fabric, engraved roll, a roller, No. two rollers and No. three rollers are arranged in coating machine, its temperature is an engraved roll: 35 ℃, No. one roller~No. three roller is 180 ℃, and temperature of oven is 110 ℃.
Embodiment four
Raw material: T32522 terylene
1, concise: the concise liquid that is mixed with by water and auxiliary agent that in the liquid bath of concise machinery, adds required amount, the composition of auxiliary agent is softener 0.3 grams per liter, surfactant 0.2 grams per liter, NaOH 5 grams per liters, desizing agent 0.6 grams per liter in metal ion chelation agent 0.1 grams per liter, the bath, Yu Weishui, after being warming up to 85 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the liquid bath that coexists, be warming up to 95 ℃ of concise temperature then, after concise 15 minutes, venting refining liquid takes out behind the adding cold water washing.
2, arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, the composition of auxiliary agent is softener 4 grams per liters, antistatic agent 0.1 grams per liter, waterproofing agent 2.0 grams per liters, Yu Weishui, after making above-mentioned refined fabric padding finishing liquid, enter again in the mechanical baking oven of arrangement, under 160 ℃ temperature, make the fabric drying typing, 35 meters/minute of the speed of a motor vehicle;
3, fluffing arrangement:, utilize the physical mechanical active force to collude silk fluffing, 15 meters/minute of the speed of a motor vehicle by the machinery that fluffs;
4, bonding: the mode of utilizing the net tube to shift, prime cement is coated on the base cloth surface with point-like equably, the spreading powdered resin is absorbed unnecessary resin then again, the place that prime cement is arranged on the base cloth is stained with or keeps resin, carry out Infrared Heating again, temperature: 180 ℃, make prime cement dry and be bonded on the base cloth surface, enter the drying room typing then, 120 ℃ of drying room temperature, 30 meters/minute of process velocities.
Embodiment five
Raw material: T32622 terylene
1, concise: the concise liquid that is mixed with by water and auxiliary agent that in the liquid bath of concise machinery, adds required amount, the composition of auxiliary agent is softener 0.1 grams per liter, surfactant 0.2 grams per liter, NaOH 4 grams per liters, desizing agent 0.3 grams per liter in metal ion chelation agent 0.1 grams per liter, the bath, Yu Weishui, after being warming up to 80 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the liquid bath that coexists, be warming up to 100 ℃ of concise temperature then, after concise 15 minutes, venting refining liquid takes out behind the adding cold water washing.
2, arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, the composition of auxiliary agent is softener 3 grams per liters, antistatic agent 0.3 grams per liter, waterproofing agent 3.0 grams per liters, Yu Weishui, after making above-mentioned refined fabric padding finishing liquid, enter again in the mechanical baking oven of arrangement, under 150 ℃ temperature, make the fabric drying typing, 30 meters/minute of the speed of a motor vehicle;
3, fluffing arrangement:, utilize the physical mechanical active force to collude silk fluffing, 25 meters/minute of the speed of a motor vehicle by the machinery that fluffs;
4, bonding: the mode of utilizing the net tube to shift, prime cement is coated on the base cloth surface with point-like equably, the spreading powdered resin is absorbed unnecessary resin then again, the place that prime cement is arranged on the base cloth is stained with or keeps resin, carry out Infrared Heating again, temperature: 170 ℃, make prime cement dry and be bonded on the base cloth surface, enter the drying room typing then, 110 ℃ of drying room temperature, 35 meters/minute of process velocities.

Claims (10)

1, Teased long staple adhesive lining cloth is characterized in that: has on the surface of fabric and utilizes the physical mechanical active force that the weft yarn of fabric is ticked one deck fine hair of breaking back formation, and the point-like resin.
2, the manufacture method of Teased long staple adhesive lining cloth is characterized in that,
Refining: refining in the High Temperature High Pressure liquid-flow dyeing machine, after being warming up to 75~85 ℃, fabric is dropped in the fluid cylinder, make water and fabric one cycle rotation in the fluid cylinder that coexists, in this process, add entry to required amount and auxiliary agent, be warming up to 90~100 ℃ of concise temperature then, after concise 5~20 minutes, venting refining liquid takes out behind the adding cold water washing;
Arrangement: in the liquid bath of arrangement machinery, add the dressing liquid that is mixed with by water and auxiliary agent, after making above-mentioned refined fabric soak into dressing liquid, enter again in the mechanical baking oven of arrangement, under 90 ℃~210 ℃ temperature, make the fabric drying typing, 25~40 meters/minute of the speed of a motor vehicle;
The fluffing arrangement: put into the fluffing arrangement mechanically through the fabric behind the arrangement mechanical finishing, utilize the physical mechanical active force that the weft yarn of fabric is ticked and break, form one deck fine hair at fabric face, its speed of a motor vehicle 10-25 rice/minute;
Bonding: make fabric after the above-mentioned fluffing arrangement through coating machine, at the bonding point-like resin of fabric face, stentering forming in stenter again, 130~180 ℃ of tentering temperature, its process velocity is: 20~45 meters/minute.
3, according to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that, the composition of the auxiliary agent in the concise liquid is softener 0.1~0.5 grams per liter, surfactant 0.1~0.5 grams per liter, NaOH 2~10 grams per liters, desizing agent 0.3~0.6 grams per liter in metal ion chelation agent 0.1~0.5 grams per liter, the bath, Yu Weishui.
4, according to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that, the composition of the auxiliary agent in the dressing liquid is softener 2~6 grams per liters, antistatic agent 0.1~1.5 grams per liter, bleeding agent 0.1~0.3 grams per liter, waterproofing agent 0.5~3.0 grams per liter, Yu Weishui.
According to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that 5, during the fluffing arrangement, the bearded needle on the utilization fluffing collator is ticked the weft yarn of fabric and broken, and carries out at normal temperatures.
According to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that 6, engraved roll, a roller, No. two rollers and No. three rollers are arranged in coating machine, its temperature is an engraved roll: 30~40 ℃, No. one roller~No. three roller is 150~210 ℃.
7, according to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that, when bonding, the mode of utilizing the net tube to shift, prime cement is coated on the fabric base cloth surface with point-like equably, and the spreading powdered resin is absorbed unnecessary resin then again, carry out Infrared Heating again, temperature: 220~270 ℃, make prime cement dry and be bonded on the fabric base cloth surface, enter drying room then and make the fabric typing, 100~140 ℃ of drying room temperature, 25~45 meters/minute of process velocities.
8, according to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that, after refining, in the high temperature liquid-flow dyeing machine, add the dye liquor of entry and auxiliary agent preparation again, under 100~150 ℃ temperature, dyeed through 20~50 minutes.
According to the manufacture method of the described Teased long staple adhesive lining cloth of claim 7, it is characterized in that 9, the addition of auxiliary agent is DISPERSE DYES 5~20 grams per liters in the dyeing, softener 0.5~1.5 grams per liter in the bath, dispersant 0.3~1 grams per liter, formic acid 0.1~0.3 grams per liter, Yu Weishui.
According to the manufacture method of the described Teased long staple adhesive lining cloth of claim 2, it is characterized in that 10,, after dyeing, soap that soaped 10~30 minutes, temperature is 70~100 ℃ in the liquid of soaping of water and soaping agent preparation; And then washing: wash in clear water, 10~20 minutes time, temperature is a normal temperature.
CN 200510040109 2005-05-18 2005-05-18 Teased long staple adhesive lining cloth and method for manufacturing same Pending CN1699666A (en)