High-insulation black organic silicon colorant and preparation method thereof
Technical Field
The application relates to the technical field of organic silicon colorants, in particular to a high-insulation black organic silicon colorant and a preparation method thereof.
Background
Black colorants are widely used in silicone materials for electronic component packaging, heat resistant coatings, insulating sealants, and other applications, and serve the function of imparting a dark appearance and visual masking to the material. In current industrial applications, black colorants mainly include inorganic pigments such as carbon black, iron black, and copper chromium black.
Among them, carbon black is the most widely used black pigment because of its extremely high tinting strength, thermal stability, and cost advantages. However, carbon black itself has high conductivity and remarkable hydrophobicity, is extremely easy to agglomerate in an organosilicon system, is difficult to uniformly disperse, and can seriously reduce the electrical insulation properties of the material. This problem is particularly pronounced in applications requiring high insulation, such as in the fields of electronic seals, insulating coatings, etc., where the product properties are significantly limited.
Although iron black (Fe 3O4) has certain coloring capability, the iron black has certain magnetism and is easy to adsorb impurity ions (such as iron ions or other conductive metal impurities), and potential electrical performance hazards exist in a system with high insulation requirements. In addition, the blackness of iron black is far lower than that of carbon black, the coloring strength is weak, and the requirements on color depth and hiding power are difficult to meet.
Although the composite oxide pigment such as copper chrome black has certain chemical stability, the tinting strength is not as good as that of carbon black and the color is grey, and the pigment is not suitable for high-end organosilicon products requiring deep black appearance. In addition, such composite oxide pigments also have application limitations in terms of fineness, wettability and system compatibility.
In summary, currently, black silicone colorants generally rely on carbon black to meet the color strength requirement when pigments are selected, but the high conductivity and agglomeration tendency of carbon black severely limit their applicability in high insulation scenes. Therefore, how to effectively solve the problems of reduced insulativity and uneven dispersion of carbon black in an organosilicon system on the premise of maintaining the deep black appearance becomes a key problem of urgent breakthrough in the field.
Disclosure of Invention
The application provides a high-insulation black organic silicon colorant and a preparation method thereof, and aims to solve the problems that the black colorant is easy to agglomerate and difficult to disperse in an organic silicon system and the electrical insulation property is obviously reduced in the prior art.
The application provides a high-insulation black organic silicon colorant which comprises, by mass, 100 parts of a silicone oil carrier, 3-5 parts of passivation carbon black and 1-3 parts of fumed silica, wherein the passivation carbon black comprises carbon black and an organic silicon layer coated on the surface of the carbon black, the organic silicon layer is obtained by graft polymerization of polymethyl triethoxysilane and a functional silane coupling agent on the surface of the carbon black, and the functional silane coupling agent comprises at least one of an aromatic silane coupling agent and a fluorine-containing silane coupling agent.
According to the application, the black coloring agent remarkably improves the electrical insulation property and dispersion stability of the black coloring agent in a silicone oil system while maintaining the advantage of high blackness of the carbon black, overcomes the problems of strong conductivity, poor interface compatibility and easy agglomeration of the carbon black, and is particularly suitable for the application of organosilicon materials with higher requirements on insulativity.
The inventor finds that the introduction of the functional silane coupling agent can further improve the dispersion stability and insulativity of the passivated carbon black in the system, and the reason is that the functional silane coupling agent can further regulate the interfacial chemical property and microstructure of the coating layer, wherein the aromatic silane coupling agent can enhance the affinity with a carbon skeleton on the surface of the carbon black through pi-pi interaction, and the introduction of the rigid skeleton and the nonpolar segment in the coating layer is beneficial to enhancing the film forming compactness of the coating layer and the anchoring stability of the carbon black, so that the dispersibility and the thermal stability of the passivated carbon black are enhanced, and the fluorine-containing silane coupling agent can introduce a fluorine-carbon structure with lower surface energy in the coating layer, further block the contact with external polar components, reduce the migration and the heavy polymerization risk of the passivated carbon black in the system, and simultaneously promote the overall resistivity of the carbon black through the high insulativity of fluorine element.
In addition, the fumed silica is introduced as inorganic nano particles with high surface activity, so that a spatially distributed network structure can be formed in the system, the network structure is distributed among carbon black particles, a certain degree of physical steric hindrance and a dispersed framework structure are formed, and the agglomeration behavior of the carbon black is limited from a microscopic level, so that the movement and the refolding trend of the carbon black are inhibited, and the system stability and the rheological control capability of the passivated carbon black in silicone oil are further improved.
The high-insulation black organic silicon colorant provided by the application has the advantages that the dispersibility, the electrical insulation property and the system stability are obviously improved on the premise of not sacrificing the color depth by the aid of the structural synergistic mechanism, and the high-insulation black organic silicon colorant is suitable for preparing black organic silicon materials with high requirements on dielectric properties.
In some embodiments, the silicone oil carrier comprises vinyl silicone oil and polyether silicone oil, wherein the mass ratio of the vinyl silicone oil to the polyether silicone oil is 9:0.5-1.5.
In some of the above embodiments, the vinyl silicone oil not only provides excellent low viscosity, heat resistance and dispersion environment as a main carrier, but also allows the vinyl groups in the molecular structure to participate in the crosslinking reaction during the subsequent heat curing or vulcanization, and undergo an addition reaction with the crosslinking agent (e.g., hydrogen-containing silane, etc.) in the silicone system, thereby being embedded in the overall silicone network structure. This feature not only helps to promote the structural integrity and mechanical strength of the system, but also locks the passivated carbon black and other components in a dispersed state during the crosslinking cure, reducing the risk of later migration or phase separation, and helping to maintain the electrical insulation stability of the colorant during use.
The hydrophilic polyether chain segment can be adsorbed in a non-coated area or microscopic gap on the surface of the passivated carbon black through Van der Waals force, polar acting force and the like to further wet the residual exposed surface to inhibit local agglomeration risk, and on the other hand, the hydrophilic polyether chain segment can also form hydrogen bond or electrostatic effect with hydroxyl on the surface of the gas phase SiO 2, so that a weak thixotropic network structure can be constructed in a system in an assisted manner, sedimentation or layering of particles can be inhibited, and storage stability and dispersion uniformity can be improved.
In addition, in the interface region between the passivated carbon blacks, the polyether silicone oil can reduce the interfacial tension between particles, so that the polyether silicone oil is distributed in a lower energy state in the system, and the processability and the interfacial adaptability of the final colorant system are improved.
When the mass ratio of the vinyl silicone oil to the polyether silicone oil is controlled within the range of 9:0.5-1.5, the dispersion synergistic effect of the polyether silicone oil can be fully exerted on the basis of ensuring the thermal stability and the subsequent crosslinkable performance of the system, and the balance of the dispersibility and the structural stability is realized, and when the proportion of the polyether silicone oil is too high, too many polar chain segments can be introduced, so that the polarity of the system is unbalanced, and the electrical insulation maintenance is not facilitated. Therefore, the silicone oil compound system not only realizes the synergy among dispersion, thixotropic and crosslinkable, but also obviously enhances the interface compatibility and stability of the colorant and the organosilicon matrix.
In some embodiments, the viscosity of the vinyl silicone oil at 25 ℃ is 350-10000 cP, and the model of the polyether silicone oil is KF-6017.
In some of the embodiments described above, control of the viscosity of the vinyl silicone oil has a significant impact on the dispersion stability and construction flexibility of the silicone colorant system. In particular, vinyl silicone oil with lower viscosity has good fluidity, but is unfavorable for stable steric hindrance after particle dispersion, while the excessive viscosity can reduce the fluidity of the colorant pre-dispersion, and initial agglomeration is easy to form. The viscosity of the vinyl silicone oil is controlled within the range of 350-10000 cP, so that good dispersion force can be provided, and meanwhile, the system is guaranteed to have good construction fluidity and thixotropic response capability, and the vinyl silicone oil is a basic condition for realizing high-efficiency dispersion and long-term stability of carbon black. By way of example, vinyl terminated dimethyl (siloxane and polysiloxane) having a viscosity of 1000cP at 25 ℃ was used as the vinyl silicone oil in one embodiment of the present application.
In addition, the polyether silicone oil is of the model KF-6017, the main chain structure of the polyether silicone oil is polydimethylsiloxane, and the side chain is grafted with a polyether chain segment, so that the polyether silicone oil has good wetting and interface spreading performance, can further reduce the interfacial tension of a system, and enhances the lubricity and particle stability of the system. The existence of polyether chain segments in KF-6017 enables the polyether chain segments to be adsorbed on the surface of carbon black or at the interface of a filler, which is not completely coated by organic silicon, and through the extension and steric hindrance effect of the flexible chain segments, the aggregation tendency caused by inter-particle van der Waals attraction is relieved, and meanwhile, an auxiliary wetting barrier is formed on the surface of passivated carbon black, so that the dispersibility of the passivated carbon black in a silicone oil carrier is improved.
In some embodiments, the method of making the passivated carbon black comprises the steps of:
S1, mixing carbon black with ethanol to disperse the carbon black in the ethanol to obtain carbon black dispersion liquid;
S2, mixing polymethyl triethoxy silane, a functional silane coupling agent and an ethanol water solution to partially hydrolyze the polymethyl triethoxy silane and the aromatic silane coupling agent to obtain a silane solution;
And S3, adding the silane solution into the carbon black dispersion liquid, and performing polycondensation crosslinking on the surface of the carbon black by using polymethyl triethoxysilane and an aryl silane coupling agent to obtain the passivated carbon black.
In some of the above embodiments, the method for preparing the passivated carbon black significantly improves the wettability and effective contact area of the carbon black surface, reduces the agglomeration degree and ensures the uniformity of subsequent silane reactions by dispersing the carbon black in a polar solvent (such as ethanol).
In the step S2, polymethyl triethoxysilane (PMTES) is used as a main crosslinking substance, a multifunctional silanol intermediate can be formed by partial hydrolysis in an ethanol aqueous solution, the crosslinking tendency is strong, and the functional silane coupling agent can be hydrolyzed to generate a silanol structure with specific functional groups, so that structural units such as aromatic rings, fluorine atoms and the like are introduced into the organic silicon shell layer in the forming process, and the shell layer is endowed with stronger interface regulation capability and microstructure stability.
In step S3, the silane solution is added to the carbon black dispersion, and the silane hydrolysate undergoes a polycondensation crosslinking reaction on the carbon black surface, thereby constructing an organosilicon shell layer on the carbon black particle surface.
The shell structure is formed by a main cross-linked reticular framework formed by PMTES and a modified functional group, so that the hydrophobic stability of carbon black particles is obviously improved, the migration and aggregation tendency of the carbon black particles in an organosilicon system is reduced, the surface conductivity of the carbon black is effectively weakened, and excellent electrical insulation performance is provided for the carbon black.
The method has simple process and easy scale, is suitable for constructing carbon black particles with good dispersibility and high insulating property, and provides ideal insulating black filler for constructing a high-insulating organosilicon colorant system.
In some embodiments, the method of making the passivated carbon black comprises the steps of:
s1, performing ultrasonic dispersion on 10 parts of carbon black in 40-60 parts of ethanol to obtain carbon black dispersion liquid;
s2, dispersing 4-6 parts of polymethyl triethoxysilane and 1-2 parts of functional silane coupling agent in 5-15 parts of ethanol water solution, and adjusting the pH to 4-5 to obtain silane solution;
and S3, adding the silane solution into the carbon black dispersion liquid, and reacting for 4-6 hours at 60-80 ℃ to obtain the passivated carbon black.
In some embodiments, the dispersion stability of the carbon black in ethanol is obviously improved in the step S1 through an ultrasonic dispersion means, agglomerated masses are effectively broken, the exposed area of the surface of the carbon black is maximized, and reaction sites are provided for the subsequent silane coating reaction.
In the step S2, polymethyl triethoxysilane is used as a main cross-linking agent, and can be rapidly hydrolyzed into a trifunctional silanol intermediate under an acidic condition (pH 4-5), and a functional silane coupling agent (such as silane with an aryl or fluoroalkyl structure) can be partially hydrolyzed under the same condition. The acidic pH control is helpful for inhibiting the silanol prepolymer from self-polycondensing in the solution, thereby improving the preferential polycondensation efficiency of the silanol prepolymer and the surface of the carbon black, and forming a directional coating structure. The addition amount of the polymethyl triethoxy silane is controlled to be 40% -60% of the mass of the carbon black, a more complete organic silicon coating layer can be formed to passivate the surface of the carbon black, and the functionalized silane coupling agent participates in the reaction in a relatively small proportion, so that the integrity and the surface energy of the organic coating layer are further improved, the agglomeration of the passivated carbon black is further inhibited, and the insulativity of the passivated carbon black is further improved.
And step S3, continuously reacting for 4-6 hours at the temperature of 60-80 ℃ to ensure that the silane hydrolysate is fully condensed and formed into a film on the surface of the carbon black, and gradually forming an organosilicon coating layer with relatively complete structure and firm adhesion. The coating layer structurally supports an integral framework by a crosslinked network formed by PMTES, and substituents introduced by functional silane regulate and control the interface polarity and flexibility of a shell layer, so that the structural passivation and the electric conductivity weakening of the carbon black surface are realized.
Through the cooperative regulation and control of the reaction parameters and the addition proportion, the integrity and the stability of the coating layer can be ensured, the secondary agglomeration of carbon black in the system is avoided, and on the other hand, the effective regulation of the electrical property of the carbon black is realized, and the construction of black functional particles with excellent dispersibility and outstanding insulativity is facilitated, so that the electrical insulation property and the long-term use stability of the organosilicon colorant system are enhanced.
In some embodiments, the polymethyltriethoxysilane has an average degree of polymerization of 2 to 3.
In some embodiments, the functional silane coupling agent comprises an aromatic silane coupling agent and a fluorine-containing silane coupling agent, and the mass ratio of the aromatic silane coupling agent to the fluorine-containing silane coupling agent is 1:0.4-0.6.
In some embodiments, the aromatic silane coupling agent has stronger pi-pi interaction capability and a certain rigid structure, can introduce a stable organic framework structure into the coating layer, enhances the anchoring capability of the shell layer and the carbon black surface, and improves the compatibility of the whole system and the organosilicon matrix. The fluorine-containing silane coupling agent can introduce a fluorocarbon chain segment with low polarity and low surface energy on the surface of the carbon black, so that a free electron conduction channel on the surface of the carbon black is effectively weakened, the conductivity of the carbon black is further inhibited from a molecular level, the introduction of an aromatic ring and fluorine also synergistically promotes the shielding effect of a group, and the compactness of a shell layer is improved.
The aryl silane and the fluorine-containing silane are cooperatively used according to the mass ratio of 1:0.4-0.6, and the insulating capacity and the interfacial energy regulating capacity of the coating layer can be further improved on the basis of improving the compactness and the structural stability of the coating shell. The proportion design can balance the surface anchoring effect of the aromatic structure and the electric insulation regulating function of the fluorocarbon chain segment, and the organosilicon coating structure with dispersion stability and high insulation performance is constructed, so that the application suitability of the passivation carbon black in an organosilicon system and the insulation performance of a final colorant can be improved.
The aromatic silane coupling agent and the fluorine-containing silane coupling agent have meanings known in the art, the aromatic silane coupling agent means a type of silane coupling agent containing an aromatic ring, and the fluorine-containing silane coupling agent means a type of silane coupling agent containing a fluoroalkyl group. By way of example, in one embodiment of the present application trifluoropropyltriethoxysilane is used as the fluorine-containing silane coupling agent.
In some embodiments, the aryl silane coupling agent comprises 4-methoxyphenyl triethoxysilane.
In some of the embodiments described above, when 4-methoxyphenyl triethoxysilane is used as the aromatic silane coupling agent, the resulting colorant has better electrical insulating properties and stability than when other phenylsilane coupling agents are used. The possible reasons are that methoxy in the 4-methoxyphenyl triethoxysilane molecule is a strong electron donating group, the electron density of a benzene ring can be obviously enhanced, so that the strength of pi-pi stacking effect between the benzene ring and the surface of carbon black is improved, the oriented adsorption and effective coverage of a coupling agent on the surface of carbon black are promoted, and meanwhile, the methoxy substituted structure also adjusts the polarity distribution of the silane coupling agent, so that the coating layer formed in the hydrolysis polycondensation process and an organosilicon resin system with weaker polarity have better interface compatibility, the energy difference at a phase interface is reduced, and the interface delamination or agglomeration tendency between the coating layer and a matrix is inhibited.
Therefore, the use of 4-methoxyphenyl triethoxysilane as an aromatic silane coupling agent can further improve the electrical insulating properties and stability of the colorant.
In some embodiments, the fumed silica has an average particle size of 10 to 50nm. Based on the above embodiment, the fumed silica with the particle size within the range has larger specific surface area and good surface activity, can form a uniformly dispersed filler network in the system, and is effectively embedded into the interfacial gap between the silicone oil matrix and the passivated carbon black. The micro-nano particle structure not only improves the distribution stability of the filler, but also forms physical partition for carbon black aggregation to a certain extent, thereby being beneficial to improving the dispersion uniformity and migration resistance of the whole system. Meanwhile, the surface hydroxyl groups of the silicone oil can form weak hydrogen bonds or association with silanol structures in a silicone oil system, so that the stability of the filler in the system is enhanced, and the electrical insulation performance and stability of the organosilicon colorant are improved.
In some embodiments, the specific surface area of the carbon black is 100-300 m 2/g. Based on the embodiment, the moderate specific surface area can ensure that the carbon black has good coloring capability and surface reactivity, thereby being beneficial to realizing more sufficient silane polycondensation cladding in the passivation process, strengthening the directional adsorption capability of the functional silane coupling agent on the basis of keeping a certain surface active site, and further enhancing the overall electrical insulation property and the coloring capability of the material.
In a second aspect, the present application provides a method of preparing a highly insulating black silicone colorant comprising:
Providing a feedstock in a high insulation black silicone colorant according to any of the embodiments of the first aspect;
And mixing the raw materials to obtain the insulating black organic silicon colorant.
According to the method, the passivated carbon black, the fumed silica and the compound silicone oil are mixed and dispersed in proportion, so that the passivated carbon black is uniformly distributed in an organic silicon system, the fumed silica is filled between the passivated carbon black and the fumed silica to form a three-dimensional supporting structure, and the silicone oil is used as a continuous phase to provide good wettability and dispersion stability. In the preparation method, the passivated carbon black is preformed into an organic silicon coating layer, so that the passivated carbon black has good interface inertia and structural stability, vinyl silicone oil in the compound silicone oil can further participate in the crosslinking reaction of base materials such as subsequent silica gel, silicone rubber and the like to realize co-curing of the system, and polyether silicone oil provides good interface blending capability to promote overall mixing uniformity. The preparation method has simple process, can be completed in conventional mixing and dispersing equipment (such as a three-roller grinder and a planetary stirrer), and is beneficial to improving the stability of products and the consistency of industrialized application.
In some embodiments, the mixing of the raw materials to obtain an insulating black silicone colorant comprises:
Dispersing the passivated carbon black in polyether silicone oil to obtain a first component;
dispersing fumed silica in vinyl silicone oil to obtain a second component;
And mixing the first component and the second component to obtain the insulating black organic silicon colorant.
Based on the above embodiments, the inventors found that the adoption of such a dispersing order can significantly enhance the synergistic distribution behavior of each component in the system while improving the dispersing efficiency. The surface polarity of the passivated carbon black is moderate, wetting and wrapping are easier to realize in the polyether silicone oil, the polyether chain segment can also form a reversible adsorption layer on the surface of the carbon black (the carbon black is not completely wrapped by an organosilicon layer in the part possibly existing in the passivated carbon black), so that particle agglomeration is further inhibited, the initial dispersion stability of a system is improved, the fumed silica has high specific surface area and abundant surface hydroxyl groups, and good physical embedding and Van der Waals effects are formed with the vinyl silicone oil, so that a continuous three-dimensional skeleton network can be constructed in the shearing and dispersing process.
In the finally mixed composite system, carbon black particles are uniformly embedded into a supporting network constructed by gas-phase SiO 2 by taking polyether silicone oil as a lubricating interface, and vinyl silicone oil and polyether silicone oil coexist in the system, so that moderate viscosity of the system and excellent workability can be ensured, a stable cross-linking structure can be formed in the subsequent organosilicon cross-linking curing process, carbon black migration, aggregation or conductive path formation can be effectively prevented, and the insulativity and service life are further improved.
Compared with the prior art, the application has the beneficial effects that:
1. According to the application, by constructing a multiphase composite system of the passivated carbon black, the fumed silica and the silicone oil carrier, the electrical insulation performance of the black organic silicon colorant is obviously improved, and the problem of dielectric breakdown or insulation failure caused by conductivity in the traditional carbon black filling system is solved;
2. According to the application, polymethyl triethoxysilane and an aryl or fluorine-containing silane coupling agent are adopted to cooperatively coat carbon black, and a compact organosilicon passivation layer with controllable electrical property is constructed by regulating and controlling the polarity, flexibility and surface energy in a coating structure, so that the black tinting strength is ensured, and meanwhile, the effective blocking of a conductive path is realized;
3. the obtained organosilicon colorant can directly participate in the crosslinking reaction of vinyl organosilicon materials, obviously improve the compatibility of the colorant and a matrix and the crosslinking embedding strength, avoid the phenomena of carbon black precipitation, color bleeding or migration, and prolong the service life of the materials.
4. The high-insulation black organic silicon colorant provided by the application has excellent electrical insulation property, dispersion stability and tinting strength, and is especially suitable for the fields of organic silicon pouring sealant, electrical packaging materials and the like with high requirements on insulation performance.
Detailed Description
Each example or embodiment in this specification is described in a progressive manner, each example focusing on differences from other examples.
In the description of the present specification, reference to the terms "one embodiment," "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples," etc., means that a particular feature, structure, material, or characteristic described in connection with the embodiment or example is included in at least one embodiment or example of the application. In this specification, schematic representations of the above terms do not necessarily refer to the same embodiments or examples. Furthermore, the particular features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.
Furthermore, the terms "first," "second," and the like, are used for descriptive purposes only and are not to be construed as indicating or implying a relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defining "a first" or "a second" may explicitly or implicitly include at least one such feature. In the description of the present application, the meaning of "plurality" means at least two, for example, two, three, etc., unless specifically defined otherwise.
In the expression of the present specification, "parts" means "parts by mass" unless otherwise specified.
Hereinafter, embodiments of the present application are described. The following examples are illustrative only and are not to be construed as limiting the application. The examples are not to be construed as limiting the specific techniques or conditions described in the literature in this field or as per the specifications of the product. The reagents or apparatus used were conventional products commercially available without the manufacturer's attention.
Vinyl silicone oil vinyl terminated dimethyl (silicone and polysiloxane) with a viscosity of 1000cP at 25 ℃;
polyether silicone oil with the model KF-6017;
The average polymerization degree of the polymethyl triethoxysilane is 2-3;
trifluoropropyl triethoxysilane with CAS number 86876-45-1;
4-methoxyphenyl triethoxysilane with CAS number of 21130-91-6;
phenyltriethoxysilane with CAS number 780-69-8;
Carbon black having a specific surface area of about 230m 2/g;
fumed silica has an average particle size of about 30nm.
Preparation example 1
Preparation of passivated carbon black:
adding 10 parts of carbon black into a reactor, adding 50 parts of ethanol, and performing ultrasonic treatment (with the frequency of 40kHz and the power of 200W) for 30min to fully disperse the carbon black to obtain carbon black dispersion liquid;
adding 5 parts of polymethyl triethoxysilane, 1 part of 4-methoxyphenyl triethoxysilane and 0.5 part of trifluoropropyl triethoxysilane into 10 parts of ethanol water solution with the ethanol volume fraction of 80%, stirring and mixing, adding acetic acid to adjust the pH to 4.5, and hydrolyzing for 30min to obtain silane solution;
And slowly dripping the silane hydrolysate into the carbon black dispersion liquid under the stirring state, heating the reaction system to 70 ℃ and preserving heat for reaction for 6 hours, naturally cooling to room temperature after the reaction is finished, centrifuging the product to obtain black solid, washing the black solid with ethanol for 3 times, and drying the black solid in a vacuum drying oven at 60 ℃ for 12 hours to obtain the passivated carbon black A with the surface passivated.
Preparation example 2
Preparation of passivated carbon black:
adding 10 parts of carbon black into a reactor, adding 50 parts of ethanol, and performing ultrasonic treatment (with the frequency of 40kHz and the power of 200W) for 30min to fully disperse the carbon black to obtain carbon black dispersion liquid;
Adding 5 parts of polymethyl triethoxysilane and 1.5 parts of 4-methoxyphenyl triethoxysilane into 10 parts of ethanol water solution with the ethanol volume fraction of 80%, stirring and mixing, adding acetic acid to adjust the pH to 4.5, and hydrolyzing for 30min to obtain silane solution;
And slowly dripping the silane hydrolysate into the carbon black dispersion liquid under the stirring state, heating the reaction system to 70 ℃ and preserving heat for reaction for 6 hours, naturally cooling to room temperature after the reaction is finished, centrifuging the product to obtain black solid, washing the black solid with ethanol for 3 times, and drying the black solid in a vacuum drying oven at 60 ℃ for 12 hours to obtain the passivated carbon black B with the surface passivated.
Preparation example 3
Preparation of passivated carbon black:
adding 10 parts of carbon black into a reactor, adding 50 parts of ethanol, and performing ultrasonic treatment (with the frequency of 40kHz and the power of 200W) for 30min to fully disperse the carbon black to obtain carbon black dispersion liquid;
adding 5 parts of polymethyl triethoxysilane and 1.5 parts of trifluoro propyl triethoxysilane into 10 parts of ethanol water solution with the ethanol volume fraction of 80%, stirring and mixing, adding acetic acid to adjust the pH to 4.5, and hydrolyzing for 30min to obtain silane solution;
Slowly dripping the silane hydrolysate into the carbon black dispersion liquid under the stirring state, heating the reaction system to 70 ℃ and preserving heat for reaction for 6 hours, naturally cooling to room temperature after the reaction is finished, centrifuging the product to obtain black solid, washing the black solid with ethanol for 3 times, and drying the black solid in a vacuum drying oven at 60 ℃ for 12 hours to obtain the passivated carbon black C with the surface passivated.
Comparative preparation example 1
Preparation of passivated carbon black:
adding 10 parts of carbon black into a reactor, adding 50 parts of ethanol, and performing ultrasonic treatment (with the frequency of 40kHz and the power of 200W) for 30min to fully disperse the carbon black to obtain carbon black dispersion liquid;
adding 6.5 parts of polymethyl triethoxysilane into 10 parts of ethanol water solution with the ethanol volume fraction of 80%, stirring and mixing, adding acetic acid to adjust the pH to 4.5, and hydrolyzing for 30min to obtain silane solution;
And slowly dripping the silane hydrolysate into the carbon black dispersion liquid under the stirring state, heating the reaction system to 70 ℃ and preserving heat for reaction for 6 hours, naturally cooling to room temperature after the reaction is finished, centrifuging the product to obtain black solid, washing the black solid with ethanol for 3 times, and drying the black solid in a vacuum drying oven at 60 ℃ for 12 hours to obtain the passivated carbon black D with the surface passivated.
Example 1
Preparation of insulating black silicone colorant:
adding 4 parts of the passivated carbon black A prepared in the preparation example 1 into 10 parts of polyether silicone oil, and dispersing 10 min at room temperature by using a high-speed shearing dispersing instrument to obtain a uniform dispersion of carbon black in the polyether silicone oil, and marking the uniform dispersion as a first component;
Adding 3 parts of fumed silica into 90 parts of vinyl silicone oil, mechanically stirring at room temperature for 5min, and then transferring into a three-roller grinder for grinding for 3 times (the roller spacing is set to 20 mu m, 10 mu m and 5 mu m) to obtain a uniformly dispersed fumed SiO 2 dispersion which is recorded as a second component;
And mixing the first component and the second component, and rotationally grinding by using zirconium beads in a grinding cavity of a sand mill for 30min to obtain the insulating black organic silicon colorant.
Example 2
Preparation of insulating black silicone colorant:
adding 4 parts of the passivated carbon black A prepared in preparation example 1 into 10 parts of vinyl silicone oil, and dispersing 10 min at room temperature by using a high-speed shearing dispersing instrument to obtain a uniform dispersion of carbon black in the vinyl silicone oil, and marking the uniform dispersion as a first component;
Adding 3 parts of fumed silica into 90 parts of vinyl silicone oil, mechanically stirring at room temperature for 5min, and then transferring into a three-roller grinder for grinding for 3 times (the roller spacing is set to 20 mu m, 10 mu m and 5 mu m) to obtain a uniformly dispersed fumed SiO 2 dispersion which is recorded as a second component;
And mixing the first component and the second component, and rotationally grinding by using zirconium beads in a grinding cavity of a sand mill for 30min to obtain the insulating black organic silicon colorant.
Example 3
Preparation of insulating black silicone colorant:
Adding 4 parts of the passivated carbon black A prepared in the preparation example 1 into 30 parts of polyether silicone oil, and dispersing 10 min at room temperature by using a high-speed shearing dispersing instrument to obtain a uniform dispersion of carbon black in the polyether silicone oil, and marking the uniform dispersion as a first component;
adding 3 parts of fumed silica into 70 parts of vinyl silicone oil, mechanically stirring at room temperature for 5min, and then transferring into a three-roller grinder for grinding for 3 times (the roller spacing is set to 20 mu m, 10 mu m and 5 mu m) to obtain a uniformly dispersed fumed SiO 2 dispersion which is recorded as a second component;
And mixing the first component and the second component, and rotationally grinding by using zirconium beads in a grinding cavity of a sand mill for 30min to obtain the insulating black organic silicon colorant.
Example 4
Preparation of insulating black silicone colorant:
The procedure is substantially as in example 1, except that the passivated carbon black B obtained in preparation example 2 is used as the passivated carbon black.
Example 5
Preparation of insulating black silicone colorant:
The same procedure as in example 1 was repeated except that the passivated carbon black C obtained in preparation example 3 was used as the passivated carbon black.
Example 6
Preparation of insulating black silicone colorant:
adding 4 parts of the passivated carbon black A prepared in preparation example 1 into 10 parts of vinyl silicone oil, and dispersing 10 min at room temperature by using a high-speed shearing dispersing instrument to obtain a uniform dispersion of carbon black in the vinyl silicone oil, and marking the uniform dispersion as a first component;
Adding 3 parts of fumed silica into 80 parts of vinyl silicone oil and 10 parts of polyether silicone oil, mechanically stirring at room temperature for 5min, and then transferring into a three-roll grinder for grinding for 3 times (roll spacing is set to 20 mu m, 10 mu m and 5 mu m) to obtain a uniformly dispersed fumed SiO 2 dispersion, and recording as a second component;
And mixing the first component and the second component, and rotationally grinding by using zirconium beads in a grinding cavity of a sand mill for 30min to obtain the insulating black organic silicon colorant.
Comparative example 1
Preparation of insulating black silicone colorant:
The same procedure as in example 1 was repeated except that the passivated carbon black D obtained in comparative preparation example 1 was used as the passivated carbon black.
Test part
Testing electrical insulation performance:
2.5g of the high insulation black silicone colorant to be tested was added to 50g of RTV-1 silicone rubber (model DONGNING 732) and repeatedly ground 3 times using a three-roll mill to uniformly disperse the colorant in the silica gel.
The ground mixture is poured into a tetrafluoro mould with the dimensions of 100mm multiplied by 1mm, and the mixture is stood for 48 hours in an environment with the temperature of 25 plus or minus 2 ℃ and the relative humidity of more than 50 percent for natural vulcanization, and after complete curing, the sample is demoulded to obtain a test sample.
Referring to GB/T1410-2006 "method for measuring volume resistivity and surface resistivity of solid insulation", a sample piece was cut into test specifications of 50 mm. Times.50 mm. Times.1 mm, upper and lower surfaces of the sample piece were clamped using a standard copper round piece electrode, volume resistivity ρ V1 (Ω. Cm) of the sample piece was measured at room temperature (25.+ -. 2 ℃) and relative humidity (50%.+ -. 2%) under 500V DC voltage, and the average value was taken for each group of 3 sample pieces, and the results are shown in Table 1.
In addition, in order to test the stability of the high-insulation black silicone colorant, the high-insulation black silicone colorant obtained in each example was placed in a 60 ℃ incubator to be stored for 15d for accelerated aging, and the high-insulation black silicone colorant after the high-temperature storage was subjected to the electrical insulation property test to test the volume resistivity ρ V2 (Ω·cm) of the corresponding sample, 3 samples were tested for each group, and the average value was taken, and the results are shown in table 1.
TABLE 1
| |
ρV1(Ω·cm) |
ρV2(Ω·cm) |
| Example 1 |
6.8×1014 |
6.7×1014 |
| Example 2 |
5.5×1014 |
5.0×1014 |
| Example 3 |
5.7×1014 |
4.9×1014 |
| Example 4 |
6.0×1014 |
5.6×1014 |
| Example 5 |
5.1×1014 |
4.6×1014 |
| Example 6 |
6.5×1014 |
6.2×1014 |
| Comparative example 1 |
3.2×1012 |
1.5×1012 |
According to table 1, ρ V1 and ρ V2 of the corresponding samples of each example are better than comparative example 1, and the storage stability of the silicone colorant can be also side-reacted by comparing the attenuation of the volume resistivity of the samples after storage, which demonstrates the beneficial effects of the high insulation black silicone colorant provided by the present application that significantly improves the volume resistivity and enhances the storage stability. The possible reason for this is that in comparative example 1, the passivation carbon black used only uses the polymethyltriethoxysilane single coating agent, and does not introduce the aromatic silane with pi-pi stacking capability or the fluorine-containing silane with interface energy regulation effect, which results in loose and uneven structure of the carbon black coating layer, and the residual conductive path between particles cannot be effectively cut off, so that the resistivity of the carbon black coating layer is significantly lower than that of each example, agglomeration easily occurs during storage, the resistivity is further reduced, and high insulation requirements are difficult to meet.
According to examples 1-3, the amount of polyether silicone oil added to the carrier has a certain effect on the dispersion stability of the passivated carbon black and the insulation performance of the system. In example 1, polyether silicone oil and vinyl silicone oil are proportionally used as carriers, and good wettability and bridging dispersion structure are provided while system compatibility is maintained, so that the colorant has the highest initial resistivity (and the lowest attenuation rate) in an RTV system, in example 2, no polyether silicone oil is added, only vinyl silicone oil is used as a carrier, the initial resistivity and the resistivity after storage are greatly reduced, the dispersion stability of the colorant is reduced when a polar wetting chain segment is lacking, in example 3, the proportion of polyether silicone oil is too high, the initial resistivity is lower than that of example 1, the attenuation rate of the resistivity is higher, and the introduction of excessive polar chain segments in the system is indicated, so that not only is electrical insulation affected, but also the polarity imbalance of the system is possibly caused, and the maintenance of electrical insulation is unfavorable.
From examples 1, 4 and 5, it is understood that the combination of the kinds of the silane coupling agents in the passivated carbon black has some influence on the insulation properties of the system. In the embodiment 1, PMTES, aromatic silane and fluorine-containing silane are compounded to form a compact coating layer with coordinated interface polarity gradient, the resistivity and the storage stability are optimal, in the embodiment 4, only the proportion of the aromatic silane is improved, the fluorine-containing component is not used, the insulation of a shell layer is reduced, the surface energy is increased, the initial resistivity and the resistivity after storage are slightly lower than those of the embodiment 1, in the embodiment 5, the fluorine-containing silane is used for replacing the aromatic silane, a pi-pi stacking auxiliary orientation layer is lacked, and the insulation and the storage stability are slightly inferior to those of the embodiment 1, so that the three-component synergistic system is most favorable for constructing the high-efficiency electric insulation shielding layer.
From examples 1 and 6, it is understood that the manner of introducing the polyether silicone oil has a certain influence on the insulating property enhancing effect of the passivated carbon black. In example 1, polyether silicone oil is directly used as a dispersion medium for dispersing passivation carbon black, and a polar chain segment of the polyether silicone oil can be preferentially adsorbed on a carbon black surface area which may be defective or not fully covered by a coating layer, so that coating compactness and an electric insulation shielding effect are further enhanced on a microscopic level, and formation of a conductive path is effectively inhibited, while in example 6, the polyether silicone oil is added into a dispersion system of fumed silica, and because of stronger hydrogen bonds and entanglement with hydroxyl groups on the surface of the fumed silica, the polyether chain segment preferentially generates a surface coating layer of the fumed silica, and complementary modification of carbon black is difficult to realize, so that the overall insulation property and storage stability of a colorant system are slightly lower than those of example 1.
It should be noted that the above embodiments are merely for illustrating the technical solution of the present application and not for limiting the same, and although the present application has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solution described in the above embodiments may be modified or some or all of the technical features may be equivalently replaced, and these modifications or substitutions do not make the essence of the corresponding technical solution deviate from the scope of the technical solution of the embodiments of the present application.