CN116789138B - A fully hollow silicon carbide microsphere and its preparation method - Google Patents

A fully hollow silicon carbide microsphere and its preparation method

Info

Publication number
CN116789138B
CN116789138B CN202310685130.2A CN202310685130A CN116789138B CN 116789138 B CN116789138 B CN 116789138B CN 202310685130 A CN202310685130 A CN 202310685130A CN 116789138 B CN116789138 B CN 116789138B
Authority
CN
China
Prior art keywords
silicon carbide
silicon
microspheres
microbeads
hollow
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN202310685130.2A
Other languages
Chinese (zh)
Other versions
CN116789138A (en
Inventor
罗建华
王健
石珂俣
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Emeishan Xinrui New Material Co ltd
Original Assignee
Emeishan Xinrui New Material Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Emeishan Xinrui New Material Co ltd filed Critical Emeishan Xinrui New Material Co ltd
Priority to CN202310685130.2A priority Critical patent/CN116789138B/en
Publication of CN116789138A publication Critical patent/CN116789138A/en
Application granted granted Critical
Publication of CN116789138B publication Critical patent/CN116789138B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种全中空碳化硅微珠及其制备方法,属于无机填料制备领域。该方法包括以下步骤:将硅粉、硅溶胶按照用量比混合,经喷雾干燥机喷雾干燥成微珠;对微珠进行包膜处理、干燥处理、固化处理和碳化处理得到碳化后的微珠;对碳化后的微珠进行烧结处理,液化的单质硅浸润外包膜,生成碳化硅外壳;内核的二氧化硅、液相硅反应生成一氧化硅气体排出,排出的一氧化硅气体与外壳包膜的碳反应生成全中空碳化硅微珠。本发明不仅解决了现有技术中制备得到的空心碳化硅微珠内核是呈蜂窝或层状的,并不是完全中空的问题,极大程度减轻了碳化硅微珠的重量,而且在此基础上有效增强了碳化硅微珠的强度,避免全中空碳化硅微珠出现破碎的问题。This invention discloses a fully hollow silicon carbide microsphere and its preparation method, belonging to the field of inorganic filler preparation. The method includes the following steps: mixing silicon powder and silica sol according to a specified ratio, and spray-drying the mixture into microspheres using a spray dryer; subjecting the microspheres to coating, drying, curing, and carbonization treatments to obtain carbonized microspheres; sintering the carbonized microspheres, where liquefied elemental silicon impregnates the outer coating to form a silicon carbide shell; the silicon dioxide and liquid silicon in the core react to generate silicon monoxide gas, which is then released. The released silicon monoxide gas reacts with the carbon coating on the outer shell to generate fully hollow silicon carbide microspheres. This invention not only solves the problem that the hollow silicon carbide microspheres prepared in the prior art have a honeycomb or layered core and are not completely hollow, greatly reducing the weight of the silicon carbide microspheres, but also effectively enhances the strength of the silicon carbide microspheres, avoiding the breakage problem of fully hollow silicon carbide microspheres.

Description

Full-hollow silicon carbide microbead and preparation method thereof
Technical Field
The invention belongs to the field of inorganic filler preparation, relates to the field of hollow microsphere preparation, and in particular relates to a full-hollow silicon carbide microsphere and a preparation method thereof.
Background
The hollow microsphere is used as a novel multifunctional material with excellent physical and chemical properties, and is used as a filler, namely, the comprehensive performance of the hollow microsphere filled into a composite material formed by other materials through a certain process can be improved by several times or even tens of times compared with that of a matrix material. The hollow silicon carbide microbeads are used in metal to replace lithium element for weight reduction and enhancement in metal, and can be used as new light and strong material without changing the original metal, such as magnesium alloy, aluminum alloy, titanium alloy, stainless steel, etc. to produce ultra-light, high-strength and low-expansion metal-based composite material. Such materials have weldability, extrudability, die-casting, castable, and other processability and can be used in the field of particular interest in weight reduction, i.e., the field of gram counts. In particular to the fields of aerospace, rocket satellites, missile patrol missiles, bulletproof armor and the like, and the method can also be used in the civil fields of unmanned aerial vehicles, electric vehicles, magnetic levitation high-speed trains and the like.
CN112047343a discloses a preparation method of hollow silicon carbide microbeads, which is to prepare porous graphite microbeads by using graphene oxide and carbon nanotubes as raw materials, coat the porous graphite microbeads with silica sol modified by a silane coupling agent, and then reinforce with silicon nitride and silicon carbide micro powder to generate compact hollow silicon carbide microbeads, so as to obtain the hollow silicon carbide microbeads with reinforced and compact surfaces. However, the problem of sufficient contact between the silicon source and the carbon source cannot be solved, so that the carbon content of the microbeads is relatively high and the strength is low.
CN1l5521162a discloses a preparation method of hollow silicon carbide microbeads, which can make lamellar graphene fully contact with silica sol, the lamellar graphene is uniformly distributed in silica gel, a silicon source and a carbon source can fully react, but the lamellar graphene is distributed in the silica sol in a lamellar or honeycomb shape, and the prepared hollow silicon carbide microbeads have honeycomb or lamellar cores and are not completely hollow.
Disclosure of Invention
The first technical problem to be solved by the invention is to provide a preparation method of the full hollow silicon carbide microbeads, and the second technical problem to be solved by the invention is to provide the full hollow silicon carbide microbeads prepared by the method.
The technical scheme adopted by the invention is as follows:
the preparation method of the full hollow silicon carbide microbeads comprises the following steps:
s1, mixing silicon powder and silica sol according to a dosage ratio, and spray-drying the mixture into microbeads by a spray dryer;
S2, coating, drying, curing and carbonizing the microbeads to obtain carbonized microbeads;
and S3, sintering the carbonized microbeads, wherein liquefied elemental silicon infiltrates the outer envelope to generate a silicon carbide shell, and silicon dioxide in the inner core reacts with liquid silicon to generate silicon monoxide gas, and the silicon monoxide gas is discharged to form the full-hollow silicon carbide microbeads.
The preparation method of the full hollow silicon carbide microbeads specifically comprises the following steps:
(1) Mixing simple substance silicon powder and silica sol according to the dosage ratio, and spray-drying into microbeads by a spray dryer;
(2) Coating the microbeads by using a coating agent to obtain coated microbeads;
(3) Placing the coated microbeads into a reaction kettle, and heating with vegetable oil as a medium to perform drying treatment and curing treatment to obtain cured microbeads;
(4) Carbonizing the solidified microbeads in a carbonization furnace to obtain carbonized microbeads;
(5) And the silicon dioxide in the inner core reacts with liquid silicon to generate silicon monoxide gas, the silicon monoxide gas is discharged, the fully hollow silicon carbide microbeads are formed, and the discharged silicon monoxide gas reacts with carbon on the surface of the shell to further generate a compact silicon carbide shell.
In some embodiments of the invention, in the step (1), simple substance silicon powder and silica sol are mixed according to the dosage ratio of 1-5:5-10.
In some embodiments of the invention, in the step (1), simple substance silicon powder and silica sol are mixed according to the dosage ratio of 1-3:2-7.
Preferably, in some embodiments of the present invention, in step (1), the elemental silicon powder and the silica sol are mixed in a ratio of 3:7.
In some embodiments of the present invention, in step (1), the silicon powder is an ultra-fine elemental silicon powder ground from polycrystalline silicon or monocrystalline silicon or metallic silicon.
In some embodiments of the present invention, in step (1), the elemental silicon powder has a particle size of 0.1 μm to 5 μm.
In some embodiments of the invention, in step (2), the coating agent is a water-soluble phenolic resin.
In some embodiments of the invention, in step (2), the coating agent is a sucrose solution.
In some embodiments of the invention, in step (3), the microbeads are dried and cured by heating with peanut oil as a medium.
In some embodiments of the present invention, in the step (3), the temperature of the drying treatment is 80 ℃ to 200 ℃, and the time of the drying treatment is 10 to 60 minutes.
In some embodiments of the present invention, in the step (3), the curing temperature is 120 to 170 ℃ and the curing time is 30 to 120 minutes.
Preferably, in some embodiments of the invention, in step (3), the curing treatment temperature is 150 ℃.
In some embodiments of the present invention, in step (4), the carbonization treatment is performed at a temperature of 800 to 1000 ℃ for a time of 60 to 180 minutes.
Preferably, in some embodiments of the invention, in step (4), the carbonization treatment is performed for a period of 70 minutes.
In some embodiments of the present invention, in step (5), the sintering process is performed at a temperature of 1400 to 2000 ℃ for a time of 2 to 6 hours.
Preferably, in some embodiments of the invention, in step (5), the sintering treatment is for a period of 5 hours.
In some embodiments of the invention, in step (5), the silicon dioxide of the inner core and the liquid silicon react at 1800 ℃ to 2000 ℃ to generate silicon monoxide gas, the silicon monoxide gas is discharged to form fully hollow silicon carbide microbeads, and the discharged silicon monoxide gas reacts with carbon on the surface of the shell to generate a compact silicon carbide shell.
The full hollow silicon carbide microbeads prepared by the method are provided.
The beneficial effects of the invention are as follows:
The invention adopts silicon and silicon dioxide as the inner core, silicon dioxide gas generated by the reduction reaction of silicon and silicon dioxide is discharged, and the discharged silicon dioxide gas reacts with carbon coated by the shell to generate the full hollow silicon carbide microbeads. The invention solves the problems that the hollow silicon carbide microbead prepared in the prior art is honeycomb or lamellar and is not completely hollow, greatly reduces the weight of the silicon carbide microbead, and on the basis, the density is lower under the same strength, thereby effectively enhancing the strength of the silicon carbide microbead and avoiding the problem that the hollow silicon carbide microbead is broken.
Detailed Description
In order to make the objects, technical solutions and advantages of the present invention more apparent, the technical solutions of the present invention will be clearly and completely described below in connection with specific embodiments of the present invention. It will be apparent that the described embodiments are only some, but not all, embodiments of the invention. All other embodiments, which can be made by those skilled in the art based on the embodiments of the invention without making any inventive effort, are intended to be within the scope of the invention. The following describes in detail the technical solutions provided by the embodiments of the present invention with reference to the embodiments.
Example 1
Grinding polycrystalline silicon (purchased from Texas crystal fire technology glass Co., ltd.) into superfine simple substance silicon powder, mixing the simple substance silicon powder with silica sol (the silica content in the silica sol is 30 percent, purchased from Zhengzhou cloud-created chemical products Co., ltd.) according to 3 g/7 mL, spray-drying into microbeads by a spray dryer, setting the temperature of a spray inlet to be 180-200 ℃, the temperature of a spray outlet to be 70-100 ℃, the spray spraying interval time to be 3-5 seconds, the spray spraying time to be 1-2 seconds, and the spray spraying air pressure to be 10-20 MPa. Mixing sucrose solution with the mass percentage of 20% with the microbeads according to the use ratio of 1:1 to obtain coated microbeads, putting the coated microbeads into a reaction kettle, heating the coated microbeads by using peanut oil as a medium to perform drying treatment and curing treatment to obtain cured microbeads, wherein the drying treatment temperature is 100 ℃, the curing treatment time is 30min, the curing treatment temperature is 140 ℃, the curing treatment time is 120min, carbonizing the cured microbeads through a carbonization furnace at 800 ℃ for 180 min to obtain carbonized microbeads, putting the carbonized microbeads into a silicon carbide sintering furnace to perform sintering treatment for 5 hours at 1800 ℃ to infiltrate the outer coating, generating a silicon carbide shell, reacting silicon dioxide of the inner core and liquid silicon at 1800-2000 ℃ to generate silicon monoxide gas, discharging the silicon carbide microbeads, and reacting the discharged silicon monoxide gas with carbon on the surface of the shell to generate a compact silicon carbide shell.
The particle size, isostatic strength and density of the fully hollow silicon carbide microbeads prepared according to JC/T2284-2014 standard test are as follows:
The particle size of the hollow silicon carbide microbeads is 10-20 um, the isostatic pressure (hydrostatic pressure) is 200mpa, and the density is 0.9g/cm 3.
Example 2
Grinding monocrystalline silicon (purchased from Texas crystal fire technology glass Co., ltd.) into superfine simple substance silicon powder, mixing the simple substance silicon powder with silica sol (the silica content in the silica sol is 30 percent, purchased from Zhengzhou cloud-created chemical products Co., ltd.) according to 3 g/7 mL, spray-drying into microbeads by a spray dryer, setting the temperature of a spray inlet to be 180-200 ℃, the temperature of a spray outlet to be 70-100 ℃, the spray spraying interval time to be 3-5 seconds, the spray spraying time to be 1-2 seconds, and the spray spraying air pressure to be 10-20 MPa. Mixing 11% water soluble phenolic resin (purity: BR) and microbeads according to a dosage ratio of 1:1 to obtain coated microbeads, placing the coated microbeads into a reaction kettle, heating with peanut oil as a medium to obtain cured microbeads, drying at 200 ℃, drying at 20min, curing at 170 ℃ for 30min, carbonizing the cured microbeads in a carbonization furnace at 1000 ℃ for 60 min to obtain carbonized microbeads, sintering the carbonized microbeads in a silicon carbide sintering furnace at 2000 ℃ for 2 hours to obtain liquefied elemental silicon to infiltrate an outer coating, forming a silicon carbide shell, reacting silicon dioxide of the inner core and liquid silicon at 1800-2000 ℃ to generate silicon oxide gas, discharging the silicon oxide gas, and reacting the discharged silicon oxide gas with the carbon shell on the surface of the shell to obtain compact silicon carbide shell.
The particle size, isostatic strength and density of the fully hollow silicon carbide microbeads prepared according to JC/T2284-2014 standard test are as follows:
The particle size of the hollow silicon carbide microbeads is 10-20 um, the isostatic pressure (hydrostatic pressure) is 200mpa, and the density is 0.9g/cm 3.
Example 3
Grinding metal silicon (purchased from Texas crystal fire technology glass Co., ltd.) into superfine simple substance silicon powder, mixing the simple substance silicon powder with silica sol (the silicon dioxide content in the silica sol is 30 percent, purchased from Zhengzhou cloud-created chemical products Co., ltd.) according to 3 g/7 mL, spray-drying into microbeads by a spray dryer, setting the temperature of a spray inlet to be 180-200 ℃, the temperature of a spray outlet to be 70-100 ℃, the spray spraying interval time to be 3-5 seconds, the spray spraying time to be 1-2 seconds, and the spray spraying air pressure to be 10-20 MPa. Mixing sucrose solution with the mass percentage of 22% and microbeads according to the use ratio of 1:1 to obtain coated microbeads, placing the coated microbeads into a reaction kettle, heating the coated microbeads by using peanut oil as a medium to perform drying treatment and curing treatment to obtain cured microbeads, wherein the drying treatment temperature is 80 ℃, the curing treatment time is 60 minutes, the curing treatment temperature is 120 ℃, the curing treatment time is 120 minutes, carbonizing the cured microbeads through a carbonization furnace at 900 ℃ for 120 minutes to obtain carbonized microbeads, placing the carbonized microbeads into a silicon carbide sintering furnace to perform sintering treatment for 4 hours at 1800 ℃ to infiltrate the outer coating, generating a silicon carbide shell, reacting silicon dioxide of the inner core and liquid silicon at 1800-2000 ℃ to generate silicon monoxide gas, discharging the silicon carbide microbeads, and reacting the discharged silicon monoxide gas with carbon on the surface of the shell to generate a compact silicon carbide shell.
The particle size, isostatic strength and density of the fully hollow silicon carbide microbeads prepared according to JC/T2284-2014 standard test are as follows:
The particle size of the hollow silicon carbide microbeads is 10-20 um, the isostatic pressure (hydrostatic pressure) is 200mpa, and the density is 0.9g/cm 3.
Comparative example 1
3-10 Layers of few-layer graphene (purchased from Anhui Mu Jia new material technology Co., ltd.) with the mass percent of 15% silica sol (the silica content of the silica sol is 30% and the silica sol is purchased from Zhengzhou cloud trauma chemical product Co., ltd.) are mixed, a 95% ethanol aqueous solution with the mass percent of 7% is added, mixed sol is obtained, and then ammonia water with the mass percent of 0.09% is added to form alcohol gel;
Then adding an ageing agent consisting of 3% of silica sol and 10% of 95% of ethanol water solution to carry out ageing treatment on the alcohol gel, wherein the ageing treatment temperature is 50 ℃ and the ageing treatment time is 14 hours, adding 14.91% of trimethylchlorosilane to carry out modification treatment, the modification treatment temperature is 50 ℃ and the modification treatment time is 120 minutes, then adding 15% of n-hexane to carry out solvent replacement treatment again, the replacement treatment temperature is 45 ℃, and the solvent replacement treatment time is 4 hours;
Then placing the alcohol gel subjected to solvent replacement treatment in a dryer for grading drying treatment, wherein the primary drying treatment temperature is 70 ℃, the primary drying treatment time is 2 hours, the secondary drying treatment temperature is 100 ℃, the secondary drying treatment time is 2 hours, the tertiary drying treatment temperature is 130 ℃, and the tertiary drying treatment time is 2 hours, so as to prepare aerogel;
Crushing the aerogel into fine aerogel particles with the particle size of 75um-100um by adopting an airflow crusher, and then treating the fine aerogel particles by adopting a spherical shaper, wherein the rotation speed of a cylindrical grinding block medium in the spherical shaper is 2500rpm, and the treatment time of the spherical shaper is 120min, so as to prepare aerogel microbeads;
Adding a 10% sucrose solution (22 g sucrose is dissolved in distilled water and the volume is fixed to 100 ml) for coating aerogel microbeads, drying by adopting an air flow dryer, wherein the inlet temperature of the air flow dryer is 250 ℃, the outlet temperature of the air flow dryer is 70 ℃, the drying time is 30 seconds, then the air flow dryer is used for curing, the curing time is 3 hours, the curing temperature is 140 ℃, the carbonization treatment is carried out in a muffle furnace, the carbonization time of the muffle furnace is 3 hours, the carbonization temperature is 500 ℃, the porous graphite microbeads are prepared, silicon powder (purchased from Shandong Texas crystal fire company) with the particle size of 3000 meshes and the mass percentage of 22% are mixed with the porous graphite microbeads, sintering is carried out in a silicon carbide sintering furnace, the sintering time is 4 hours, and the sintering temperature is 1800 ℃ to prepare the hollow silicon carbide microbeads.
The particle size, isostatic strength and density of the hollow silicon carbide microbeads prepared according to JC/T2284-2014 standard test are as follows:
The particle size of the hollow silicon carbide microbeads is 75-100um, the isostatic pressure (hydrostatic pressure) is 140Mpa, and the density is 0.5g/cm < 3 >.

Claims (9)

1.一种全中空碳化硅微珠的制备方法,其特征在于,包括以下步骤:1. A method for preparing fully hollow silicon carbide microspheres, characterized by comprising the following steps: S1、将硅粉、硅溶胶按照用量比混合,经喷雾干燥机喷雾干燥成微珠;S1. Mix silicon powder and silica sol according to the dosage ratio, and then spray dry them into microbeads using a spray dryer; S2、对微珠进行包膜处理、干燥处理、固化处理和碳化处理得到碳化后的微珠;S2. The microspheres are coated, dried, cured and carbonized to obtain carbonized microspheres. S3、对碳化后的微珠进行烧结处理,液化的单质硅浸润外包膜,生成碳化硅外壳;内核的二氧化硅、液相硅反应生成一氧化硅气体排出,形成全中空的碳化硅微珠;S3. The carbonized microspheres are sintered, and the liquefied elemental silicon wets the outer film to form a silicon carbide shell; the silicon dioxide and liquid silicon in the core react to generate silicon monoxide gas, which is then discharged to form a completely hollow silicon carbide microsphere. 所述步骤S1中,所述硅粉为单质硅粉;单质硅粉的平均粒径为0.1μm~5μm。In step S1, the silicon powder is elemental silicon powder; the average particle size of the elemental silicon powder is 0.1 μm to 5 μm. 2.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S1中,将硅粉、硅溶胶按照用量比为1~5:2~10混合。2. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S1, silicon powder and silica sol are mixed in a ratio of 1-5:2-10. 3.根据权利要求2所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S1中,将硅粉、硅溶胶按照用量比为1~3:2~7混合。3. The method for preparing fully hollow silicon carbide microspheres according to claim 2, characterized in that, in step S1, silicon powder and silica sol are mixed in a ratio of 1-3:2-7. 4.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S2中,采用包覆剂对微珠进行包膜处理,所述包覆剂为水溶性酚醛树脂和蔗糖溶液中的一种。4. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S2, the microspheres are coated with a coating agent, wherein the coating agent is one of water-soluble phenolic resin and sucrose solution. 5.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S2中,对微珠进行干燥处理和固化处理时,用花生油作为媒介加热进行干燥处理、固化处理,干燥处理的温度为80℃~200℃,干燥处理的时间为0~60min;固化处理的温度为120~170℃,固化处理的时间为30~120min。5. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S2, when drying and curing the microspheres, peanut oil is used as a medium for heating to perform the drying and curing treatments, the drying temperature is 80℃~200℃, and the drying time is 0~60min; the curing temperature is 120~170℃, and the curing time is 30~120min. 6.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S2中,碳化处理的温度为800~1000℃,碳化处理的时间为60~180min。6. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S2, the carbonization temperature is 800-1000℃ and the carbonization time is 60-180min. 7.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S3中,烧结处理的温度为1400~2000℃,烧结处理的时间为2~6h。7. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S3, the sintering temperature is 1400-2000℃ and the sintering time is 2-6h. 8.根据权利要求1所述的全中空碳化硅微珠的制备方法,其特征在于,步骤S3中,内核的二氧化硅、单质硅在1800℃~2000℃下反应生成一氧化硅气体排出,形成全中空的碳化硅微珠;排出的一氧化硅气体与外壳表面的碳反应生成致密的碳化硅外壳。8. The method for preparing fully hollow silicon carbide microspheres according to claim 1, characterized in that, in step S3, the silicon dioxide and elemental silicon in the core react at 1800℃~2000℃ to generate silicon monoxide gas, which is then discharged to form fully hollow silicon carbide microspheres; the discharged silicon monoxide gas reacts with the carbon on the surface of the outer shell to generate a dense silicon carbide outer shell. 9.权利要求1至8任一项所述方法制备得到的全中空碳化硅微珠。9. Hollow silicon carbide microspheres prepared by the method according to any one of claims 1 to 8.
CN202310685130.2A 2023-06-09 2023-06-09 A fully hollow silicon carbide microsphere and its preparation method Active CN116789138B (en)