CN114798724A - High-speed wire rod and large-coil composite wire and production method - Google Patents
High-speed wire rod and large-coil composite wire and production method Download PDFInfo
- Publication number
- CN114798724A CN114798724A CN202210505834.2A CN202210505834A CN114798724A CN 114798724 A CN114798724 A CN 114798724A CN 202210505834 A CN202210505834 A CN 202210505834A CN 114798724 A CN114798724 A CN 114798724A
- Authority
- CN
- China
- Prior art keywords
- rolling
- finishing
- wire rod
- sizing
- reducing
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明涉及一种高速线材及大盘卷复合线及生产方法,属于钢铁冶金工业长材生产技术领域,包括共用段,以及与其相连的高速线材段和大盘卷段;共用段包括沿轧制方向顺次设置的坯料加热装置、粗轧机组、粗轧机组后飞剪、中轧机组、中轧后水冷装置、中轧机组后飞剪;高速线材段包括沿轧制方向顺次设置的预精轧机组、预精轧后水冷装置、精轧一组、精轧二组、精轧后水冷装置、减定径机组、减定径后水冷装置、高速飞剪、吐丝机前夹送辊及吐丝机、风冷线、集卷及收集系统;大盘卷段包括沿轧制方向顺次设置的精轧机组、精轧后水冷装置、飞剪、减定径机组、减定径后水冷装置、收集系统。本发明实现了高速线材与大盘卷的共线生产,降低了投资及运行成本。
The invention relates to a high-speed wire rod and a large coil composite line and a production method, belonging to the technical field of long material production in the iron and steel metallurgical industry, comprising a common section, and a high-speed wire rod section and a large coil section connected thereto; Subsequently set billet heating device, rough rolling group, rear flying shear of rough rolling group, intermediate rolling group, water cooling device after intermediate rolling, and rear flying shear of intermediate rolling group; Unit, water cooling device after pre-finishing rolling, one group of finishing rolling, two groups of finishing rolling, water cooling device after finishing rolling, reducing and sizing unit, water cooling device after reducing and sizing, high-speed flying shear, front pinch roll of laying machine and spout Wire machine, air-cooling line, collecting coil and collecting system; the large coil section includes finishing rolling line set in sequence along the rolling direction, water cooling device after finishing rolling, flying shear, reducing and sizing unit, water cooling device after reducing and sizing, collection system. The invention realizes the co-linear production of the high-speed wire rod and the large coil, and reduces the investment and operation cost.
Description
技术领域technical field
本发明属于钢铁冶金工业长材生产技术领域,涉及一种高速线材及大盘卷复合线及生产方法。The invention belongs to the technical field of long product production in the iron and steel metallurgy industry, and relates to a high-speed wire rod and a large coil composite wire and a production method.
背景技术Background technique
线棒材作为钢铁行业的重要产品之一,广泛用于汽车、机械及金属制品行业。近年来,产量持续增加。As one of the important products in the steel industry, wire rods are widely used in the automobile, machinery and metal products industries. Production has continued to increase in recent years.
1)高速线材生产线1) High-speed wire rod production line
高速线材生产线主轧线轧制机组主要包括:粗轧机组、中轧机组、预精轧机组、精轧机组和减定径机组。目前,高速线材粗轧机组、中轧机组、预精轧机组、精轧机组和减定径机组机架数一般分别为6架+6架+6架+8架+4架,若无减定径则轧线轧机数量一般为28架(6架+6架+6架+10架)。粗轧、中轧一般为短应力线轧机;预精轧机组一般为短应力线轧机或90°顶交悬臂轧机,也有部分产线采用45°顶交悬臂轧机,精轧机组及减定径机组均采用45°顶交悬臂轧机。The main rolling line rolling unit of the high-speed wire rod production line mainly includes: rough rolling unit, intermediate rolling unit, pre-finishing rolling unit, finishing rolling unit and reducing and sizing unit. At present, the number of high-speed wire rod roughing mills, intermediate rolling mills, pre-finishing mills, finishing mills and reducing and sizing mills is generally 6+6+6+8+4 frames respectively. The number of rolling mills in the diameter rolling line is generally 28 (6 frames + 6 frames + 6 frames + 10 frames). Rough rolling and intermediate rolling are generally short stress line rolling mills; pre-finishing mills are generally short stress line rolling mills or 90° top-cross cantilever rolling mills, and some production lines use 45° top-cross cantilever rolling mills, finishing rolling mills and reducing sizing mills All use 45° top-cross cantilever rolling mills.
2)大盘卷生产线2) Large coil production line
大盘卷生产线主轧线轧制机组主要包括:粗轧机组、中轧机组、精轧机组和减定径机组。目前大盘卷粗轧机组、中轧机组、精轧机组和减定径机组机架数一般分别为6架+6架+6架+4架,若无减定径则轧线轧机数量一般为18架(6架+6架+6架)。粗轧、中轧、精轧一般为短应力线轧机;减定径一般为三辊轧机,也有部分产线采用预应力式短应力线轧机。The main rolling line rolling unit of the large coil production line mainly includes: rough rolling unit, intermediate rolling unit, finishing rolling unit and reducing and sizing unit. At present, the number of stands of large coil roughing mill, intermediate rolling mill, finishing mill and reducing and sizing mill is generally 6+6+6+4, if there is no reduction and sizing, the number of rolling mills is generally 18 racks (6 racks + 6 racks + 6 racks). Rough rolling, intermediate rolling, and finishing rolling are generally short-stress line rolling mills; reducing and sizing are generally three-high rolling mills, and some production lines use prestressed short-stress line rolling mills.
随着客户对钢铁产品性能要求的提高及钢铁厂对成本控制的需求提高,为了获得更优的力学性能,需要采用全线低温轧制,然而,目前高速线材精轧机组及减定径机组采用45°顶交悬臂轧机,轧制大规格产品时轧机不稳定,无法实现低温轧制,均采用850℃以上温度轧制。With the improvement of customer's performance requirements for steel products and the increasing demand of steel mills for cost control, in order to obtain better mechanical properties, it is necessary to adopt low-temperature rolling across the entire line. °Top cross cantilever rolling mill, the rolling mill is unstable when rolling large-size products, and it is impossible to achieve low-temperature rolling, all of which are rolled at temperatures above 850 °C.
部分大盘卷生产线配备了三辊减定径机组,然而目前配备三辊减定径机组的大盘卷生产线,产线速度低均不超过18m/s,导致轧线小时产量低。Some large coil production lines are equipped with a three-roll reduction and sizing unit. However, the current large coil production line equipped with a three-roll reduction and sizing unit has a low production line speed of less than 18m/s, resulting in a low hourly output of the rolling line.
另外,高速线材生产线、大盘卷生产线为分线布置,不能实现二者的共线成产,产线柔性不足,使得投资及运行成本较高。In addition, the high-speed wire rod production line and the large coil production line are arranged in separate lines, which cannot realize the co-production of the two, and the flexibility of the production line is insufficient, which makes the investment and operation cost high.
发明内容SUMMARY OF THE INVENTION
有鉴于此,本发明的目的在于提供一种高速线材及大盘卷复合线及生产方法,以实现高速线材与大盘卷的共线生产。In view of this, the purpose of the present invention is to provide a high-speed wire rod and a large coil composite wire and a production method, so as to realize the co-linear production of the high-speed wire rod and the large coil.
为达到上述目的,本发明提供如下技术方案:For achieving the above object, the present invention provides the following technical solutions:
一种高速线材及大盘卷复合线,包括共用段,以及与其相连的高速线材段和大盘卷段;共用段:包括沿轧制方向顺次设置的坯料加热装置、粗轧机组、粗轧机组后飞剪、中轧机组、中轧后水冷装置、中轧机组后飞剪;高速线材段:包括沿轧制方向顺次设置的预精轧机组、预精轧后水冷装置、精轧一组、精轧二组、精轧后水冷装置、减定径机组、减定径后水冷装置、高速飞剪、吐丝机前夹送辊及吐丝机、风冷线、集卷及收集系统;大盘卷段:包括沿轧制方向顺次设置的精轧机组、精轧后水冷装置、飞剪、减定径机组、减定径后水冷装置、收集系统;高速线材段的精轧一组为三辊轧机组、精轧二组为45°顶交悬臂轧机组,减定径机组为45°顶交悬臂轧机组;大盘卷段的减定径机组为三辊轧机组。A high-speed wire rod and large coil composite line, comprising a common section, and a high-speed wire rod section and a large coil section connected thereto; the common section includes a billet heating device, a rough rolling group, and a rear section of the rough rolling group arranged in sequence along the rolling direction. Flying shear, intermediate rolling unit, water cooling device after intermediate rolling, flying shear after intermediate rolling unit; high-speed wire rod section: including pre-finishing rolling unit, water-cooling device after pre-finishing rolling, one group of finishing rolling, Two groups of finishing rolling, water cooling device after finishing rolling, reducing and sizing unit, water cooling device after reducing and sizing, high-speed flying shear, front pinch roll and laying head of laying machine, air cooling line, coil collecting and collecting system; Coil section: including finishing rolling unit, water cooling device after finishing rolling, flying shear, reducing and sizing unit, water cooling device after reducing and sizing, and collecting system arranged in sequence along the rolling direction; The rolling mill and the second finishing mill are 45° top-cross cantilever rolling mills, and the reducing and sizing mills are 45° top-crossing cantilever mills; the reducing and sizing mills of the large coil section are three-roll mills.
可选地,粗轧机组与中轧机组采用连续轧制时,粗轧机组与中轧机组之间为粗轧后飞剪;粗轧机组与中轧机组采用脱头轧制时,粗轧机组与中轧机组之间为脱头辊道及粗轧后飞剪。Optionally, when the rough rolling group and the intermediate rolling group adopt continuous rolling, the rough rolling group and the intermediate rolling group use flying shears after rough rolling; Between it and the intermediate rolling unit are the stripping roller table and the flying shear after rough rolling.
可选地,脱头辊道包括保温辊道及补热装置。Optionally, the deheading roller table includes a heat preservation roller table and a heat supplement device.
可选地,高速线材段的精轧一组与大盘卷段的减定径机组为同一机组。Optionally, the finishing rolling group of the high-speed wire rod segment and the diameter reducing and sizing group of the large coil segment are the same group.
可选地,中轧后水冷装置的长度范围为10m~80m;对于高速线材段,预精轧后水冷装置的长度范围为20m~80m;精轧后水冷装置的长度范围为30m~100m;减定径后水冷装置的长度范围为15m~50m;对于大盘卷段,精轧后水冷装置的长度范围为20m~80m;减定径后水冷装置的长度范围为15m~100m。Optionally, the length range of the water cooling device after intermediate rolling is 10m to 80m; for the high-speed wire rod section, the length range of the water cooling device after pre-finishing is 20m to 80m; the length of the water cooling device after finishing rolling is 30m to 100m; The length of the water cooling device after sizing is 15m to 50m; for large coil sections, the length of the water cooling device after finishing rolling is 20m to 80m; the length of the water cooling device after reduction and sizing is 15m to 100m.
一种高速线材及大盘卷生产方法,提供上述所述的复合线,对于高速线材段,生产直径≤12mm的小规格产品时,选择减定径机组出成品,轧件进减定径机组的温度≥700℃;生产直径≥12mm的大规格产品时,选择45°顶交悬臂式减定径机组或三辊式精轧机组出成品;当选择45°顶交悬臂式减定径机组出成品时,轧件进出成品的机架的温度≥850℃;当选择三辊式精轧机组出成品时,轧件进出成品的机架的温度≥700℃;对于大盘卷段,选择三辊式减径机机组出成品,轧件进出成品的机架的温度≥700℃。A method for producing high-speed wire rods and large coils, which provides the above-mentioned composite wire. For high-speed wire rod segments, when producing small-sized products with a diameter of ≤12 mm, a reduction and sizing unit is selected to produce finished products, and the rolling stock is fed into the temperature of the sizing unit. ≥700℃; When producing large-size products with diameter ≥12mm, choose 45° top-cross cantilever type reducing and sizing unit or three-roll finishing mill to produce finished products; when choosing 45° top-cross cantilever type reducing and sizing unit to produce finished products , the temperature of the stand where the rolling stock enters and leaves the finished product is greater than or equal to 850 °C; when the three-roll finishing mill is selected to output the finished product, the temperature of the rolling stock entering and exiting the finished product is greater than or equal to 700 °C; The temperature of the stand where the rolling stock enters and exits the finished product is greater than or equal to 700 ℃.
可选地,高速线材段的精轧一组的单道次延伸率为1.10~1.35。Optionally, the single-pass elongation of one group of finishing rolling of the high-speed wire rod segment is 1.10-1.35.
可选地,大盘卷段的减定径机组的单道次延伸率为1.10~1.35,最后一架的延伸率<1.20。Optionally, the single-pass elongation rate of the reducing and sizing unit of the large coil section is 1.10-1.35, and the elongation rate of the last frame is less than 1.20.
可选地,对于高速线材段,生产直径≥12mm的大规格产品时,采用三辊式精轧机组出成品,精轧机出口速度≥50m/s。Optionally, for high-speed wire rod segments, when producing large-size products with a diameter of ≥ 12 mm, a three-roll finishing mill is used to produce finished products, and the exit speed of the finishing mill is ≥ 50 m/s.
可选地,高速线材段的产品直径范围为Φ4.5mm~Φ28.0mm,大盘卷段的产品直径范围为Φ12.0mm~Φ50.0mm。Optionally, the product diameter of the high-speed wire segment ranges from Φ4.5mm to Φ28.0mm, and the product diameter of the large coil segment ranges from Φ12.0mm to Φ50.0mm.
本发明的有益效果在于:The beneficial effects of the present invention are:
1)实现了包含高速线材及大盘卷所有规格范围内的全规格低温轧制;1) Realized full-scale low-temperature rolling in all specifications including high-speed wire rods and large coils;
2)高速线材通过二辊减定径机组或三辊精轧机出成品,产品尺寸精度高;大盘卷通过三辊减定径出成品,产品尺寸精度高;2) The high-speed wire rod passes through the two-roll reduction and sizing unit or the three-roll finishing mill to produce the finished product, and the product has high dimensional accuracy; the large coil passes through the three-roll reduction and sizing to produce the finished product, and the product has high dimensional accuracy;
3)采用低温大压下轧制,可以通过相变强化提高优特钢线材及大盘卷材的综合力学性能。生产的产品性能优异,组织稳定,具有较好的发展前景,符合绿色环保、可持续发展目标;3) Rolling at low temperature and high pressure can improve the comprehensive mechanical properties of excellent and special steel wire rods and large coils through phase transformation strengthening. The products produced have excellent performance, stable organization, good development prospects, and meet the goals of green environmental protection and sustainable development;
4)通过低温轧制细化晶粒,降低了优特钢轧制及后续精整工序时的热处理成本,降低了全流程投资及运行成本,提高了生产的稳定性,提高了经济效益;4) The grain refinement through low-temperature rolling reduces the heat treatment cost of special steel rolling and subsequent finishing processes, reduces the investment and operation cost of the whole process, improves the stability of production, and improves economic benefits;
5)生产稳定,产线的产量高,与普通高速线材相比,12mm规格高速线材速度可达到50m/s,小时产量提高10%;5) The production is stable and the output of the production line is high. Compared with ordinary high-speed wire, the speed of 12mm high-speed wire can reach 50m/s, and the hourly output is increased by 10%;
6)与普通高速线材相比,大规格可采用三辊精轧机组出成品,实现了大规格高速线材的低温轧制,解决了目前高速线材生产线无法实现大规格低温轧制的问题;6) Compared with ordinary high-speed wire rods, the three-roll finishing mill can be used to produce finished products with large specifications, which realizes the low-temperature rolling of large-scale high-speed wire rods, and solves the problem that the current high-speed wire rod production lines cannot achieve large-scale low-temperature rolling;
7)产品生产规格范围广,可以生产Φ4.5mm~Φ50.0mm规格范围内所有产品,其中高速线材段的产品直径范围为Φ4.5mm~Φ28.0mm,大盘卷段的产品直径范围为Φ12.0mm~Φ50.0mm。7) The product has a wide range of production specifications, and can produce all products within the specification range of Φ4.5mm~Φ50.0mm. Among them, the product diameter range of the high-speed wire segment is Φ4.5mm~Φ28.0mm, and the product diameter of the large coil segment is Φ12. 0mm~Φ50.0mm.
本发明的其他优点、目标和特征在某种程度上将在随后的说明书中进行阐述,并且在某种程度上,基于对下文的考察研究对本领域技术人员而言将是显而易见的,或者可以从本发明的实践中得到教导。本发明的目标和其他优点可以通过下面的说明书来实现和获得。Other advantages, objects, and features of the present invention will be set forth in the description that follows, and will be apparent to those skilled in the art based on a study of the following, to the extent that is taught in the practice of the present invention. The objectives and other advantages of the present invention may be realized and attained by the following description.
附图说明Description of drawings
为了使本发明的目的、技术方案和优点更加清楚,下面将结合附图对本发明作优选的详细描述,其中:In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be preferably described in detail below with reference to the accompanying drawings, wherein:
图1为本发明高速线材及大盘卷复合线布置示意图;Fig. 1 is the layout schematic diagram of the high-speed wire rod and the large coil composite wire of the present invention;
图2为本发明的小规格高速线材典型规格孔型系统图;Fig. 2 is the typical specification hole pattern system diagram of the small-sized high-speed wire rod of the present invention;
图3为本发明的中规格高速线材典型规格孔型系统图,其中,图3a为不经三辊精轧机或二辊精轧机,二辊减定径出成品,图3b为经三辊精轧机或二辊精轧机,二辊减定径出成品;Fig. 3 is a typical specification pass system diagram of a medium-sized high-speed wire rod according to the present invention, wherein Fig. 3a shows the finished product without passing through a three-roll finishing mill or a two-roll finishing mill, and Fig. 3b shows the finished product through a three-roll finishing mill Or two-roll finishing mill, and the finished product is produced by reducing the diameter of the two-roller;
图4为本发明的大规格高速线材典型规格孔型系统图,其中,图4a为三辊精轧机出成品,图4b为二辊减定径出成品;Fig. 4 is the typical specification pass system diagram of the large-sized high-speed wire rod according to the present invention, wherein, Fig. 4a is the finished product produced by the three-roll finishing mill, and Fig. 4b is the finished product produced by the two-roller reducing and sizing;
图5为本发明的大盘卷典型规格孔型系统图;Fig. 5 is the typical specification hole pattern system diagram of the large coil of the present invention;
图6为本发明的高速线材低温控轧温度曲线;Fig. 6 is the low temperature controlled rolling temperature curve of the high-speed wire rod of the present invention;
图7为本发明的大盘卷低温控轧温度曲线。Fig. 7 is the temperature curve of the low temperature controlled rolling of the large coil of the present invention.
附图标记:加热装置1、粗轧机组2、粗轧机组后飞剪3、中轧机组4、中轧后水冷装置5、中轧机组后飞剪6、高速线材段预精轧机组7-1、高速线材段预精轧后水冷装置8-1、高速线材段飞剪9-1、高速线材段精轧一组10-1、高速线材段精轧二组11-1、高速线材段精轧后水冷装置12-1、高速线材段飞剪13-1、高速线材段减定径机组14-1、高速线材段减定径后水冷装置15-1、高速线材段飞剪16-1、高速线材段吐丝机前夹送辊及吐丝机17-1、高速线材段风冷线18-1、高速线材段集卷及收集系统19-1、大盘卷段精轧机组7-2、大盘卷段精轧后水冷装置8-2、大盘卷段飞剪9-2、大盘卷段减定径机组10-2、大盘卷段减定径后水冷装置11-2、大盘卷段卷取机12-2、大盘卷段移卷机13-2、共用PF线及后续收集装置14-2。Reference numerals: heating device 1,
具体实施方式Detailed ways
以下通过特定的具体实例说明本发明的实施方式,本领域技术人员可由本说明书所揭露的内容轻易地了解本发明的其他优点与功效。本发明还可以通过另外不同的具体实施方式加以实施或应用,本说明书中的各项细节也可以基于不同观点与应用,在没有背离本发明的精神下进行各种修饰或改变。需要说明的是,以下实施例中所提供的图示仅以示意方式说明本发明的基本构想,在不冲突的情况下,以下实施例及实施例中的特征可以相互组合。The embodiments of the present invention are described below through specific specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the drawings provided in the following embodiments are only used to illustrate the basic idea of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
其中,附图仅用于示例性说明,表示的仅是示意图,而非实物图,不能理解为对本发明的限制;为了更好地说明本发明的实施例,附图某些部件会有省略、放大或缩小,并不代表实际产品的尺寸;对本领域技术人员来说,附图中某些公知结构及其说明可能省略是可以理解的。Among them, the accompanying drawings are only used for exemplary description, and represent only schematic diagrams, not physical drawings, and should not be construed as limitations of the present invention; in order to better illustrate the embodiments of the present invention, some parts of the accompanying drawings will be omitted, The enlargement or reduction does not represent the size of the actual product; it is understandable to those skilled in the art that some well-known structures and their descriptions in the accompanying drawings may be omitted.
本发明实施例的附图中相同或相似的标号对应相同或相似的部件;在本发明的描述中,需要理解的是,若有术语“上”、“下”、“左”、“右”、“前”、“后”等指示的方位或位置关系为基于附图所示的方位或位置关系,仅是为了便于描述本发明和简化描述,而不是指示或暗示所指的装置或元件必须具有特定的方位、以特定的方位构造和操作,因此附图中描述位置关系的用语仅用于示例性说明,不能理解为对本发明的限制,对于本领域的普通技术人员而言,可以根据具体情况理解上述术语的具体含义。The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar components; in the description of the present invention, it should be understood that if there are terms “upper”, “lower”, “left” and “right” , "front", "rear" and other indicated orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the indicated device or element must be It has a specific orientation, is constructed and operated in a specific orientation, so the terms describing the positional relationship in the accompanying drawings are only used for exemplary illustration, and should not be construed as a limitation of the present invention. situation to understand the specific meaning of the above terms.
请参阅图1~图7,一种高速线材及大盘卷复合线,包括共用段,以及与其相连的高速线材段和大盘卷段;共用段:包括沿轧制方向顺次设置的坯料加热装置1、粗轧机组2、粗轧机组后飞剪3、中轧机组4、中轧后水冷装置5、中轧机组后飞剪6;高速线材段:包括沿轧制方向顺次设置的高速线材段预精轧机组7-1、高速线材段预精轧后水冷装置8-1、高速线材段飞剪9-1、高速线材段精轧一组10-1、高速线材段精轧二组11-1、高速线材段精轧后水冷装置12-1、高速线材段飞剪13-1、高速线材段减定径机组14-1、高速线材段减定径后水冷装置15-1、高速线材段飞剪16-1、高速线材段吐丝机前夹送辊及吐丝机17-1、高速线材段风冷线18-1、高速线材段集卷及收集系统19-1、共用PF线及后续收集装置14-2;大盘卷段:包括沿轧制方向顺次设置的大盘卷段精轧机组7-2、大盘卷段精轧后水冷装置8-2、大盘卷段飞剪9-2、大盘卷段减定径机组10-2、大盘卷段减定径后水冷装置11-2、大盘卷段卷取机12-2、大盘卷段移卷机13-2、共用PF线及后续收集装置14-2;高速线材段的精轧一组可选择三辊轧机组、精轧二组可选择45°顶交悬臂轧机组,减定径机组可选择45°顶交悬臂轧机组;大盘卷段的减定径机组可选择三辊轧机组。Please refer to Figures 1 to 7, a high-speed wire rod and large coil composite line, including a common section, and a high-speed wire rod section and a large coil section connected to it; the common section: including the billet heating device 1 arranged in sequence along the rolling direction , Rough rolling
可选地,粗轧机组与中轧机组采用连续轧制时,粗轧机组与中轧机组之间为粗轧后飞剪;粗轧机组与中轧机组采用脱头轧制时,粗轧机组与中轧机组之间为脱头辊道及粗轧后飞剪。Optionally, when the rough rolling group and the intermediate rolling group adopt continuous rolling, the rough rolling group and the intermediate rolling group use flying shears after rough rolling; Between it and the intermediate rolling unit are the stripping roller table and the flying shear after rough rolling.
可选地,脱头辊道包括保温辊道及补热装置。Optionally, the deheading roller table includes a heat preservation roller table and a heat supplement device.
可选地,高速线材段的精轧一组与大盘卷段的减定径机组为同一机组。Optionally, the finishing rolling group of the high-speed wire rod segment and the diameter reducing and sizing group of the large coil segment are the same group.
可选地,中轧后水冷装置的长度范围为10m~80m;对于高速线材段,预精轧后水冷装置的长度范围为20m~80m;精轧后水冷装置的长度范围为30m~100m;减定径后水冷装置的长度范围为15m~50m;对于大盘卷段,精轧后水冷装置的长度范围为20m~80m;减定径后水冷装置的长度范围为15m~100m。Optionally, the length range of the water cooling device after intermediate rolling is 10m to 80m; for the high-speed wire rod section, the length range of the water cooling device after pre-finishing is 20m to 80m; the length of the water cooling device after finishing rolling is 30m to 100m; The length of the water cooling device after sizing is 15m to 50m; for large coil sections, the length of the water cooling device after finishing rolling is 20m to 80m; the length of the water cooling device after reduction and sizing is 15m to 100m.
一种高速线材及大盘卷生产方法,提供上述所述的复合线,对于高速线材段,生产直径≤12mm的小规格产品时,选择减定径机组出成品,轧件进减定径机组的温度≥700℃;生产直径≥12mm的大规格产品时,选择45°顶交悬臂式减定径机组或三辊式精轧机组出成品;当选择45°顶交悬臂式减定径机组出成品时,轧件进出成品的机架的温度≥850℃;当选择三辊式精轧机组出成品时,轧件进出成品的机架的温度≥700℃;对于大盘卷段,选择三辊式减径机机组出成品,轧件进出成品的机架的温度≥700℃。A method for producing high-speed wire rods and large coils, which provides the above-mentioned composite wire. For high-speed wire rod segments, when producing small-sized products with a diameter of ≤12 mm, a reduction and sizing unit is selected to produce finished products, and the rolling stock is fed into the temperature of the sizing unit. ≥700℃; When producing large-size products with diameter ≥12mm, choose 45° top-cross cantilever type reducing and sizing unit or three-roll finishing mill to produce finished products; when choosing 45° top-cross cantilever type reducing and sizing unit to produce finished products , the temperature of the stand where the rolling stock enters and leaves the finished product is greater than or equal to 850 °C; when the three-roll finishing mill is selected to output the finished product, the temperature of the rolling stock entering and exiting the finished product is greater than or equal to 700 °C; The temperature of the stand where the rolling stock enters and exits the finished product is greater than or equal to 700 ℃.
本发明的高速线材段的产品直径范围为Φ4.5mm~Φ28.0mm,大盘卷段的产品直径范围为Φ12.0mm~Φ50.0mm。对于高速线材段,生产直径≥12mm的大规格产品时,采用三辊式精轧机组出成品,精轧机出口速度≥50m/s。The product diameter of the high-speed wire segment of the present invention ranges from Φ4.5mm to Φ28.0mm, and the product diameter of the large coil segment ranges from Φ12.0mm to Φ50.0mm. For high-speed wire rod section, when producing large-size products with diameter ≥12mm, three-roll finishing mill is used to produce finished products, and the exit speed of finishing mill is ≥50m/s.
具体地:specifically:
1)高速线材1) High-speed wire
(1)加热:采用步进梁式加热装置将钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat the billet to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为850℃~1200℃;(2) Rough rolling mill rolling: The heated billet is subjected to 6 passes of short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. Shape rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system, the average elongation of the pass deformation during the rolling process is 1.20 ~ 1.40, and the deformation temperature is 850 ℃ ~ 1200 °C;
(3)中轧机组轧制:对经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为820℃~1100℃;(3) Rolling in the middle rolling mill: 6 passes of the rolling mill after rough rolling and flying shearing head and tail are carried out, and the pass system during rolling is an ellipse-circular pass system. During the rolling process, the average elongation of the pass deformation is 1.20~1.40, and the deformation temperature is 820℃~1100℃;
(4)中轧后控制冷却:对经中轧后的轧件进行控制水冷并回复;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling;
(5)预精轧机组轧制:对经中轧后控制冷却后,并经飞剪切头尾后的轧件进行6道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为800℃~1050℃;(5) Pre-finishing mill rolling: 6 passes of short stress line or cantilever mill pre-finishing mill rolling is performed on the rolled pieces after intermediate rolling and controlled cooling, and after flying shearing head and tail. The pass system is an ellipse-circular pass system, the average elongation of the pass deformation during the rolling process is 1.20-1.40, and the deformation temperature is 800℃-1050℃;
(6)预精轧后控制冷却:对经预精轧轧制后的轧件进行控制水冷并回复;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolling stock after pre-finishing rolling;
(7)三辊式精轧一组轧制:对经预精轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次三辊式精轧机组轧制,轧制时孔型系统为弧三角-弧三角-弧三角-弧三角孔型系统,轧制过程中道次变形平均延伸率为1.10~1.35,变形温度为780℃~950℃;(7) One-group rolling of three-roll finishing rolling: 4 passes of three-roll finishing rolling are performed on the rolling stock that has been pre-finished and then controlled and cooled, and has been subjected to flying shearing at the head and tail. The pass system is arc triangle-arc triangle-arc triangle-arc triangle pass system, the average elongation of pass deformation during rolling is 1.10~1.35, and the deformation temperature is 780℃~950℃;
(8)二辊式精轧机组轧制:对经三辊式精轧一组轧制后的轧件进行4道次45°顶交悬臂精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,,轧制过程中道次变形平均延伸率为1.10~1.35,变形温度为800℃~950℃;(8) Two-roll finishing mill rolling: 4 passes of 45° top-cross cantilever finishing rolling are performed on the rolling stock after one group of three-roll finishing rolling, and the pass system is elliptical during rolling. - Round pass system, the average elongation of the pass deformation during the rolling process is 1.10 ~ 1.35, and the deformation temperature is 800 ° C ~ 950 ° C;
(9)精轧后控制冷却:对经精轧轧制后的轧件进行控制水冷并回复;(9) Controlled cooling after finishing rolling: Controlled water cooling and recovery of the rolled piece after finishing rolling;
(10)减定径机组轧制:对经精轧后控制冷却的轧件进行4道次45°顶交悬臂减定径机组轧制,轧制时孔型系统为椭圆-圆-圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.05~1.30,变形温度为750℃~900℃;(10) Rolling by reducing and sizing unit: 4 passes of 45° top-cross cantilever reducing and sizing unit rolling is performed on the rolled pieces after finishing rolling, and the pass system during rolling is ellipse-circle-circle-circle Pass system, the average elongation of the pass deformation during the rolling process is 1.05~1.30, and the deformation temperature is 750℃~900℃;
(11)减定径后控制冷却:对经减定径轧制后的轧件进行控制水冷并回复;(11) Controlled cooling after reduction and sizing: control water cooling and recovery of the rolled piece after reduction and sizing;
(12)吐丝、风冷线控制冷却及收集:对经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为700℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(12) Controlled cooling and collection of wire laying and air-cooling line: The rolling stock that has been reduced and sizing is controlled to be cooled by pinch feeding. The laying temperature is 700°C to 1000°C. , Different steel grades have different controlled cooling processes. The average cooling rate of the air-cooled line ranges from 0.1 °C/s to 30 °C/s. ℃, PF line cooling is carried out after the roll is collected, and it is weighed and collected after being packaged.
2)大盘卷2) Large coil
(1)加热:采用步进梁式加热装置将钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat the billet to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为850℃~1200℃;(2) Rough rolling mill rolling: The heated billet is subjected to 6 passes of short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. Shape rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system, the average elongation of the pass deformation during the rolling process is 1.20 ~ 1.40, and the deformation temperature is 850 ℃ ~ 1200 °C;
(3)中轧机组轧制:对经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为820℃~1100℃;(3) Rolling in the middle rolling mill: 6 passes of the rolling mill after rough rolling and flying shearing head and tail are carried out, and the pass system during rolling is an ellipse-circular pass system. During the rolling process, the average elongation of the pass deformation is 1.20~1.40, and the deformation temperature is 820℃~1100℃;
(4)中轧后控制冷却:对经中轧后的轧件进行控制水冷并回复;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling;
(5)精轧机组轧制:对经中轧后控制冷却后,并经飞剪切头尾后的轧件进行6道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,轧制过程中道次变形平均延伸率为1.20~1.40,变形温度为800℃~1050℃;(5) Finishing rolling mill rolling: 6 passes of short stress line or cantilever rolling mill pre-finishing mill rolling is performed on the rolling stock that has been controlled and cooled after intermediate rolling, and has been subjected to flying shearing at the head and tail. The shape system is an ellipse-round hole system, the average elongation of the pass deformation during the rolling process is 1.20 ~ 1.40, and the deformation temperature is 800 ° C ~ 1050 ° C;
(6)精轧后控制冷却:对经精轧轧制后的轧件进行控制水冷并回复;(6) Controlled cooling after finishing rolling: Controlled water cooling and recovery of the finished rolling stock;
(7)三辊减定径机组轧制:对经精轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次三辊式减定径机组轧制,轧制时孔型系统为弧三角-弧三角-弧三角-弧三角孔型系统,轧制过程中道次变形平均延伸率为1.10~1.35,最后一架的延伸率<1.20,变形温度为750℃~950℃;(7) Three-roll reduction and sizing unit rolling: 4 passes of three-roll reduction and sizing unit rolling are performed on the rolled pieces after finishing rolling, controlled cooling, and flying shearing of the head and tail. The shape system is arc triangle-arc triangle-arc triangle-arc triangle pass system, the average elongation of the pass deformation during the rolling process is 1.10~1.35, the elongation of the last frame is less than 1.20, and the deformation temperature is 750℃~950℃ ;
(8)减定径后控制冷却:对经减定径轧制后的轧件进行控制水冷并回复;(8) Controlled cooling after reduction and sizing: control water cooling and recovery of the rolled piece after reduction and sizing;
(9)卷取机卷曲、收集:对经减定径后控制冷却的轧件进行卷曲,卷曲温度为700℃~1000℃,卷曲后进行PF线冷却,经打包后称重收集。(9) Coiler coiling and collection: Coil the rolled pieces that have been reduced and sizing and controlled to be cooled. The coiling temperature is 700°C to 1000°C. After coiling, PF line cooling is performed, and after being packaged, it is weighed and collected.
此种生产线及生产方法,与传统生产线及生产方法相比,可以实现包含高速线材及大盘卷所有规格范围内的全规格低温轧制,高速线材通过二辊减定径机组或三辊精轧机出成品,产品尺寸精度高;大盘卷通过三辊减定径出成品,产品尺寸精度高;采用低温大压下轧制,可以通过相变强化提高优特钢线材及大盘卷材综合力学性能。生产的产品性能优异,组织稳定。通过低温轧制细化晶粒,降低优特钢轧制及后续精整工序时的热处理成本,降低全流程投资及运行成本,提高生产稳定性,提高经济效益;产线生产稳定,产线产量高,与普通高速线材相比,12mm规格高速线材速度可达到50m/s,小时产量提高10%;与普通高速线材相比,大规格可采用三辊精轧机组出成品,实现低温轧制,解决了目前高速线材生产线无法实现低温轧制的问题;本发明的生产线可以生产Φ4.5mm~Φ50.0mm规格范围内所有产品,其中高速线材段的产品直径范围为Φ4.5mm~Φ28.0mm,大盘卷段的产品直径范围为Φ12.0mm~Φ50.0mm。Compared with the traditional production line and production method, this kind of production line and production method can realize full-scale low-temperature rolling in all specifications including high-speed wire rods and large coils. The finished product has high dimensional accuracy; the large coil is produced by three-roller reduction and sizing, and the product has high dimensional accuracy; the use of low temperature and large reduction rolling can improve the comprehensive mechanical properties of excellent special steel wire rod and large coil coil through phase transformation strengthening. The products produced have excellent performance and stable organization. The grain refinement through low-temperature rolling reduces the heat treatment cost of special steel rolling and subsequent finishing processes, reduces the investment and operation cost of the whole process, improves production stability, and improves economic efficiency; the production line is stable and the output of the production line is stable. Compared with ordinary high-speed wire rod, the speed of 12mm high-speed wire rod can reach 50m/s, and the hourly output is increased by 10%; The problem that the current high-speed wire rod production line cannot realize low-temperature rolling is solved; the production line of the present invention can produce all products within the specification range of Φ4.5mm~Φ50.0mm, and the product diameter range of the high-speed wire rod segment is Φ4.5mm~Φ28.0mm, The product diameter of the large coil section ranges from Φ12.0mm to Φ50.0mm.
实施例1——Φ6.0mm小规格高速线材Example 1 - Φ6.0mm small size high-speed wire
表1本发明高速线材各规格轧制速度及小时产量Table 1 The rolling speed and hourly output of each specification of the high-speed wire rod of the present invention
参照图1、图2、图6与表1,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、预精轧机组轧制、预精轧后水冷及回复、精轧前飞剪切头尾、三辊式精轧一组轧制、二辊式精轧二组轧制、精轧后水冷及回复、减定径机组轧制、减定径后水冷及回复、高速飞剪剪头尾、吐丝机前夹送辊夹送及吐丝成圈、风冷线控制冷却、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 2, Fig. 6 and Table 1, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shearing head and tail after intermediate rolling, pre-finishing rolling, water cooling and recovery after pre-finishing, flying shearing head and tail before finishing, three-roll finishing rolling, one group rolling, two-roll rolling Two sets of finishing rolling, water cooling and recovery after finishing rolling, rolling by reducing and sizing unit, water cooling and recovery after reducing and sizing, high-speed flying shear shearing head and tail, pinch roll in front of laying machine, and laying into a loop , Air-cooled line to control cooling, volume and collection. The process is as follows:
(1)加热:采用步进梁式加热装置将截面尺寸为160mm×160mm的钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat a billet with a cross-sectional size of 160mm×160mm to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.346,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.121m/s,6V机架的出口速度为0.72m/s,经6道次轧制完成后轧件等效直径为75mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.346, and the deformation temperature is 850℃~1200℃. The exit speed of the 6V stand is 0.72m/s, and the equivalent diameter of the rolled piece after 6 passes of rolling is 75mm;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.289,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为0.72m/s,12V机架的出口速度为3.32m/s,经6道次轧制完成后轧件直径为35mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the head and tail of the flying shearing is subjected to 6 passes of rolling in the middle rolling mill, and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.289, the deformation temperature is 820 ° C ~ 1100 ° C, the bite of the 7H stand during the rolling process of the middle rolling mill The speed is 0.72m/s, the exit speed of the 12V stand is 3.32m/s, and the diameter of the rolled piece is 35mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)预精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行6道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.253,变形温度为800℃~1050℃,预精轧机组轧制过程中13H机架的咬入速度为3.32m/s,18V机架的出口速度为12.83m/s,经6道次轧制完成后轧件直径为17.8mm;(5) Pre-finishing mill rolling: After controlling the cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 6 passes of short stress line or cantilever mill pre-finishing mill rolling. , The pass system during rolling is an elliptical-circular pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.253, and the deformation temperature is 800℃~1050℃. During the rolling process of the rolling mill, the bite speed of the 13H stand is 3.32m/s, the exit speed of the 18V stand is 12.83m/s, and the diameter of the rolled piece after 6 passes of rolling is 17.8mm;
(6)预精轧后控制冷却:对步骤(5)经预精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolled piece after pre-finishing rolling in step (5), and the temperature drop range of a single water tank is 50°C to 200°C;
(7)三辊式精轧一组轧制:对步骤(6)经预精轧后控制冷却后,并经飞剪切头尾后的轧件进行进行4道次三辊式精轧机组轧制,轧制时孔型系统为弧三角-弧三角-弧三角-弧三角孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.255,变形温度为780℃~950℃,精轧机组轧制过程中19#机架的咬入速度为12.83m/s,22#机架的出口速度为31.84m/s,经4道次轧制完成后轧件直径为11.3mm;(7) One group of three-roll finishing rolling: After pre-finishing in step (6), the rolling stock after the pre-finishing is controlled and cooled, and the rolling stock after the head and tail is cut by flying is subjected to 4-pass three-roll finishing rolling. During rolling, the pass system is arc triangle-arc triangle-arc triangle-arc triangle pass system. There are guide guards before and after each rolling mill. During the rolling process, the average elongation of pass deformation is 1.255. It is 780℃~950℃. During the rolling process of the finishing mill, the bite speed of the 19# stand is 12.83m/s, and the exit speed of the 22# stand is 31.84m/s. The diameter of the piece is 11.3mm;
(8)二辊式精轧机组轧制:对步骤(7)经三辊式精轧一组轧制后的轧件进行4道次45°顶交悬臂精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.253,变形温度为800℃~950℃,预精轧机组轧制过程中23#机架的咬入速度为31.84m/s,26#机架的出口速度为78.42m/s,经4道次轧制完成后轧件直径为7.2mm;(8) Two-high finishing rolling mill rolling: 4 passes of 45° top-crossing cantilever finishing rolling mill rolling is performed on the rolled piece after one group of three-high finishing rolling in step (7). The forming system is an ellipse-circular pass type system. There are guides before and after each rolling mill. The average elongation of the pass deformation during the rolling process is 1.253, and the deformation temperature is 800℃~950℃. The rolling process of the pre-finishing rolling unit The bite speed of the middle 23# stand is 31.84m/s, the exit speed of the 26# stand is 78.42m/s, and the diameter of the rolled piece after 4 passes of rolling is 7.2mm;
(9)精轧后控制冷却:对步骤(8)经精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(9) Controlled cooling after finishing rolling: the rolling stock after finishing rolling in step (8) is subjected to controlled water cooling and recovery, and the temperature drop range of a single water tank is 50°C to 200°C;
(10)减定径机组轧制:对步骤(7)经精轧后控制冷却的轧件进行4道次45°顶交悬臂减定径机组轧制,轧制时孔型系统为椭圆-圆-圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.088,变形温度为750℃~900℃,减定径机组轧制过程中27#机架的咬入速度为78.42m/s,30#机架的出口速度为110m/s,经4道次轧制完成后轧件直径为6.0mm;(10) Rolling by reducing and sizing unit: 4 passes of 45° top-cross cantilever reducing and sizing unit rolling is performed on the rolled piece that has been controlled and cooled after finishing rolling in step (7), and the pass system during rolling is ellipse-circle -Round-round pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.088, and the deformation temperature is 750℃~900℃. #The bite speed of the stand is 78.42m/s, the exit speed of the 30# stand is 110m/s, and the diameter of the rolled piece after 4 passes of rolling is 6.0mm;
(11)减定径后控制冷却:对步骤(10)经减定径轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(11) Controlled cooling after reducing and sizing: Controlling water-cooling and recovery of the rolling stock after reducing and sizing rolling in step (10), the temperature drop range of a single water tank is 50°C to 200°C;
(12)吐丝、风冷线控制冷却及收集:对步骤(11)经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为700℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(12) Controlled cooling and collection of wire laying and air-cooling lines: pinch and lay the rolled piece that has been controlled and cooled after reducing and sizing in step (11). The cooling line is controlled for cooling. Different steel grades control the cooling process differently. The average cooling rate of the air-cooled line ranges from 0.1℃/s to 30℃/s. 400 ℃ ~ 550 ℃, PF line cooling after collection, weighing and collecting after packaging.
实施例2——Φ14.0mm中规格高速线材(不经三辊精轧机或二辊精轧机,二辊减定径出成品)Example 2 - Φ14.0mm medium-sized high-speed wire rod (without the three-roll finishing mill or the two-roll finishing mill, the finished product is produced by reducing the diameter of the two-roller)
参照图1、图3、图6与表1,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、预精轧机组轧制、预精轧后水冷及回复、精轧后水冷及回复、减定径机组轧制、减定径后水冷及回复、高速飞剪剪头尾、吐丝机前夹送辊夹送及吐丝成圈、风冷线控制冷却、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 3, Fig. 6 and Table 1, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shear head and tail after intermediate rolling, pre-finishing mill rolling, water cooling and recovery after pre-finishing, water cooling and recovery after finishing rolling, rolling by reducing and sizing unit, water cooling and recovery after reducing and sizing, High-speed flying shears, cutting head and tail, pinch rolls in front of laying machine and laying into loops, air-cooling line controlled cooling, coiling and collection. The process is as follows:
(1)加热:采用步进梁式加热装置将截面尺寸为160mm×160mm的钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat a billet with a cross-sectional size of 160mm×160mm to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.346,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.233m/s,6V机架的出口速度为1.38m/s,经6道次轧制完成后轧件等效直径为75mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.346, and the deformation temperature is 850℃~1200℃. The exit speed of the 6V stand is 1.38m/s, and the equivalent diameter of the rolling stock is 75mm after 6 passes of rolling;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.289,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为1.38m/s,12V机架的出口速度为6.35m/s,经6道次轧制完成后轧件直径为35mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the head and tail of the flying shearing is subjected to 6 passes of rolling in the middle rolling mill, and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.289, the deformation temperature is 820 ° C ~ 1100 ° C, the bite of the 7H stand during the rolling process of the middle rolling mill The speed is 1.38m/s, the exit speed of the 12V stand is 6.35m/s, and the diameter of the rolled piece is 35mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)预精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行6道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.253,变形温度为800℃~1050℃,预精轧机组轧制过程中13H机架的咬入速度为6.35m/s,16V机架的出口速度为24.55m/s,经6道次轧制完成后轧件直径为17.8mm;(5) Pre-finishing mill rolling: After controlling the cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 6 passes of short stress line or cantilever mill pre-finishing mill rolling. , The pass system during rolling is an elliptical-circular pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.253, and the deformation temperature is 800℃~1050℃. During the rolling process of the rolling mill, the bite speed of the 13H stand is 6.35m/s, the exit speed of the 16V stand is 24.55m/s, and the diameter of the rolled piece after 6 passes of rolling is 17.8mm;
(6)预精轧后控制冷却:对步骤(5)经预精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolled piece after pre-finishing rolling in step (5), and the temperature drop range of a single water tank is 50°C to 200°C;
(7)精轧后控制冷却:对步骤(6)经预精轧后控制冷却后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(7) Controlled cooling after finishing rolling: The rolling stock after the controlled cooling after pre-finishing rolling in step (6) is controlled by water cooling and recovered, and the temperature drop range of a single water tank is 50°C to 200°C;
(8)减定径机组轧制:对步骤(7)经精轧后控制冷却的轧件进行4道次45°顶交悬臂减定径机组轧制,轧制时孔型系统为椭圆-圆-圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.120,变形温度为750℃~900℃,减定径机组轧制过程中27#机架的咬入速度为24.55m/s,30#机架的出口速度为38.70m/s,经4道次轧制完成后轧件直径为14.0mm;(8) Rolling by reducing and sizing unit: 4 passes of 45° top-cross cantilever reducing and sizing unit rolling is performed on the rolled piece that has been controlled and cooled after finishing rolling in step (7), and the pass system during rolling is ellipse-circle -Round-round pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.120, and the deformation temperature is 750℃~900℃. # The bite speed of the stand is 24.55m/s, the exit speed of the 30# stand is 38.70m/s, and the diameter of the rolled piece after 4 passes of rolling is 14.0mm;
(9)减定径后控制冷却:对步骤(8)经减定径轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(9) Controlled cooling after reducing and sizing: The rolling stock after reducing and sizing rolling in step (8) is controlled for water cooling and recovery, and the temperature drop range of a single water tank is 50°C to 200°C;
(10)吐丝、风冷线控制冷却及收集:对步骤(9)经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为700℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(10) Controlled cooling and collection of wire laying and air-cooling lines: pinch and lay the rolled piece that has been controlled and cooled after reducing and sizing in step (9). The cooling line is controlled by the cooling line. Different steel grades control the cooling process differently. The average cooling rate of the air-cooled line ranges from 0.1°C/s to 30°C/s. 400 ℃ ~ 550 ℃, PF line cooling after collection, weighing and collecting after packaging.
实施例3——Φ14.0mm中规格高速线材(经三辊精轧机或二辊精轧机,二辊减定径出成品)Example 3 - Φ14.0mm medium-sized high-speed wire rod (through a three-roll finishing mill or a two-roll finishing mill, the finished product is produced by reducing the diameter of the two-roller)
参照图1、图3、图6与表1,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、预精轧机组轧制、预精轧后水冷及回复、精轧后水冷及回复、减定径机组轧制、减定径后水冷及回复、高速飞剪剪头尾、吐丝机前夹送辊夹送及吐丝成圈、风冷线控制冷却、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 3, Fig. 6 and Table 1, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shear head and tail after intermediate rolling, pre-finishing mill rolling, water cooling and recovery after pre-finishing, water cooling and recovery after finishing rolling, rolling by reducing and sizing unit, water cooling and recovery after reducing and sizing, High-speed flying shears, cutting head and tail, pinch rolls in front of laying machine and laying into loops, air-cooling line controlled cooling, coiling and collection. The process is as follows:
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.346,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.233m/s,6V机架的出口速度为1.38m/s,经6道次轧制完成后轧件等效直径为75mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.346, and the deformation temperature is 850℃~1200℃. The exit speed of the 6V stand is 1.38m/s, and the equivalent diameter of the rolling stock is 75mm after 6 passes of rolling;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.289,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为1.38m/s,12V机架的出口速度为6.35m/s,经6道次轧制完成后轧件直径为35mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the flying shearing head and tail is rolled in the middle rolling mill in 6 passes, and the pass system during rolling is ellipse-circle For the pass system, there are guides before and after each rolling mill. The average elongation of the pass deformation during the rolling process is 1.289, and the deformation temperature is 820℃~1100℃. The speed is 1.38m/s, the exit speed of the 12V stand is 6.35m/s, and the diameter of the rolled piece is 35mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)预精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.256,变形温度为800℃~1050℃,预精轧机组轧制过程中13H机架的咬入速度为6.35m/s,16V机架的出口速度为15.79m/s,经4道次轧制完成后轧件直径为22.2mm;(5) Pre-finishing rolling unit rolling: After controlling the cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 4 passes of short stress line or cantilever rolling mill pre-finishing rolling unit rolling , The pass system during rolling is an ellipse-circular pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.256, and the deformation temperature is 800℃~1050℃. During the rolling process of the rolling mill, the bite speed of the 13H stand is 6.35m/s, the exit speed of the 16V stand is 15.79m/s, and the diameter of the rolled piece after 4 passes of rolling is 22.2mm;
(6)预精轧后控制冷却:对步骤(5)经预精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolled piece after pre-finishing rolling in step (5), and the temperature drop range of a single water tank is 50°C to 200°C;
(7)三辊式精轧一组或二辊式精轧二组轧制:对步骤(6)经预精轧后控制冷却后,并经飞剪切头尾后的轧件进行2道次三辊式精轧机组或二辊式精轧二组轧制,三辊式精轧机组轧制时孔型系统为弧三角-弧三角孔型系统,二辊式精轧机组轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.247,变形温度为750℃~950℃,精轧机组轧制过程中咬入速度为15.79m/s,出口速度为24.55m/s,经2道次轧制完成后轧件直径为17.8mm;(7) One group of three-roll finishing rolling or two groups of two-roll finishing rolling: After pre-finishing in step (6), the rolling stock after pre-finishing is controlled for cooling, and the rolling stock after the head and tail is cut by flying is subjected to two passes. Three-high finishing mill or two-high finishing mill rolling, the pass system of three-high finishing mill is arc triangle-arc triangle pass system, and the pass system of two-high finishing mill is rolling. The system is an ellipse-round pass system, with guides before and after each rolling mill. The average elongation of the pass deformation during the rolling process is 1.247, and the deformation temperature is 750℃~950℃. The entry speed is 15.79m/s, the exit speed is 24.55m/s, and the diameter of the rolled piece is 17.8mm after 2 passes of rolling;
(8)精轧后控制冷却:对步骤(7)经预精轧后控制冷却后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(8) Controlled cooling after finishing rolling: The rolling stock after pre-finishing rolling and controlled cooling in step (7) is controlled to be water-cooled and recovered, and the temperature drop range of a single water tank is 50°C to 200°C;
(9)减定径机组轧制:对步骤(8)经精轧后控制冷却的轧件进行4道次45°顶交悬臂减定径机组轧制,轧制时孔型系统为椭圆-圆-圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.120,变形温度为750℃~900℃,减定径机组轧制过程中27#机架的咬入速度为24.55m/s,30#机架的出口速度为38.70m/s,经4道次轧制完成后轧件直径为14.0mm;(9) Rolling by reducing and sizing unit: 4 passes of 45° top-crossing cantilever reducing and sizing unit rolling is performed on the rolling stock after finishing rolling in step (8), and the pass system during rolling is ellipse-circle -Round-round pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.120, and the deformation temperature is 750℃~900℃. # The bite speed of the stand is 24.55m/s, the exit speed of the 30# stand is 38.70m/s, and the diameter of the rolled piece after 4 passes of rolling is 14.0mm;
(10)减定径后控制冷却:对步骤(9)经减定径轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(10) Controlled cooling after reducing and sizing: The rolling stock after reducing and sizing rolling in step (9) is controlled by water cooling and recovered, and the temperature drop range of a single water tank is 50°C to 200°C;
(11)吐丝、风冷线控制冷却及收集:对步骤(10)经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为700℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(11) Controlled cooling and collection of spinning and air-cooling lines: pinch spinning and spinning of the rolling stock that has been controlled and cooled after reducing and sizing in step (10). The spinning temperature is 700°C to 1000°C. The cooling line is controlled by the cooling line. Different steel grades control the cooling process differently. The average cooling rate of the air-cooled line ranges from 0.1°C/s to 30°C/s. 400 ℃ ~ 550 ℃, PF line cooling after collection, weighing and collecting after packaging.
实施例4——Φ20.0mm大规格高速线材(三辊精轧机出成品)Example 4 - Φ20.0mm large-scale high-speed wire rod (finished product from three-roller finishing mill)
参照图1、图4、图6与表1,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、预精轧机组轧制、预精轧后水冷及回复、精轧前飞剪切头尾、三辊式精轧一组轧制、精轧后水冷及回复、减定径后水冷及回复、高速飞剪剪头尾、吐丝机前夹送辊夹送及吐丝成圈、风冷线控制冷却、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 4, Fig. 6 and Table 1, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shearing head and tail after intermediate rolling, pre-finishing rolling, water cooling and recovery after pre-finishing, flying shearing head and tail before finishing, three-roll finishing rolling in one group, after finishing Water cooling and recovery, water cooling and recovery after reducing and sizing, high-speed flying shears, cutting head and tail, pinch rolls in front of the laying machine and laying and looping, air cooling line control cooling, collecting and collecting. The process is as follows:
(1)加热:采用步进梁式加热装置将截面尺寸为160mm×160mm的钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat a billet with a cross-sectional size of 160mm×160mm to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.346,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.233m/s,6V机架的出口速度为1.38m/s,经6道次轧制完成后轧件等效直径为75mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.346, and the deformation temperature is 850℃~1200℃. The exit speed of the 6V stand is 1.38m/s, and the equivalent diameter of the rolling stock is 75mm after 6 passes of rolling;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.289,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为1.38m/s,12V机架的出口速度为6.35m/s,经6道次轧制完成后轧件直径为35mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the head and tail of the flying shearing is subjected to 6 passes of rolling in the middle rolling mill, and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.289, the deformation temperature is 820 ° C ~ 1100 ° C, the bite of the 7H stand during the rolling process of the middle rolling mill The speed is 1.38m/s, the exit speed of the 12V stand is 6.35m/s, and the diameter of the rolled piece is 35mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)预精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.183,变形温度为800℃~1050℃,预精轧机组轧制过程中13H机架的咬入速度为6.35m/s,16V机架的出口速度为12.45m/s,经4道次轧制完成后轧件直径为25.0mm;(5) Pre-finishing rolling unit rolling: After controlling the cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 4 passes of short stress line or cantilever rolling mill pre-finishing rolling unit rolling , The pass system during rolling is an elliptical-circular pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.183, and the deformation temperature is 800 ℃ ~ 1050 ℃. During the rolling process of the rolling mill, the bite speed of the 13H stand is 6.35m/s, the exit speed of the 16V stand is 12.45m/s, and the diameter of the rolled piece after 4 passes of rolling is 25.0mm;
(6)预精轧后控制冷却:对步骤(5)经预精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolled piece after pre-finishing rolling in step (5), and the temperature drop range of a single water tank is 50°C to 200°C;
(7)三辊式精轧一组轧制:对步骤(6)经预精轧后控制冷却后,并经飞剪切头尾后的轧件进行进行4道次三辊式精轧机组轧制,轧制时孔型系统为弧三角-弧三角-弧三角-弧三角孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.111,变形温度为750℃~950℃,精轧机组轧制过程中19#机架的咬入速度为12.45m/s,22#机架的出口速度为18.90m/s,经4道次轧制完成后轧件直径为20.0mm;(7) One group of three-roll finishing rolling: After pre-finishing in step (6), the rolling stock after the pre-finishing is controlled and cooled, and the rolling stock after the head and tail is cut by flying is subjected to 4-pass three-roll finishing rolling. During rolling, the pass system is arc triangle-arc triangle-arc triangle-arc triangle pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of pass deformation is 1.111. 750℃~950℃, the bite speed of 19# stand is 12.45m/s and the exit speed of 22# stand is 18.90m/s during the rolling process of finishing mill. The diameter of the piece is 20.0mm;
(9)精轧后控制冷却:对步骤(7)经精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50~200℃;(9) Controlled cooling after finishing rolling: the rolling stock after finishing rolling in step (7) is subjected to controlled water cooling and recovery, and the temperature drop range of a single water tank is 50-200 °C;
(10)减定径后控制冷却:对步骤(9)经精轧后控制冷却的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(10) Controlled cooling after reduction and sizing: Controlled water cooling and recovery of the rolled piece after finishing rolling in step (9), the temperature drop range of a single water tank is 50°C to 200°C;
(11)吐丝、风冷线控制冷却及收集:对步骤(10)经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为700℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(11) Controlled cooling and collection of spinning and air-cooling lines: pinch spinning and spinning of the rolling stock that has been controlled and cooled after reducing and sizing in step (10). The spinning temperature is 700°C to 1000°C. The cooling line is controlled for cooling. Different steel grades control the cooling process differently. The average cooling rate of the air-cooled line ranges from 0.1℃/s to 30℃/s. 400 ℃ ~ 550 ℃, PF line cooling after collection, weighing and collecting after packaging.
实施例5——Φ20.0mm大规格高速线材(二辊减定径出成品)Example 5 - Φ20.0mm large-scale high-speed wire (two-roller reduction and sizing to produce finished products)
参照图1、图4、图6与表1,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、预精轧机组轧制、预精轧后水冷及回复、精轧前飞剪切头尾、三辊式精轧一组轧制、二辊式精轧二组轧制、精轧后水冷及回复、减定径机组轧制、减定径后水冷及回复、高速飞剪剪头尾、吐丝机前夹送辊夹送及吐丝成圈、风冷线控制冷却、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 4, Fig. 6 and Table 1, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shearing head and tail after intermediate rolling, pre-finishing rolling, water cooling and recovery after pre-finishing, flying shearing head and tail before finishing, three-roll finishing rolling, one group rolling, two-roll rolling Two sets of finishing rolling, water cooling and recovery after finishing rolling, rolling by reducing and sizing unit, water cooling and recovery after reducing and sizing, high-speed flying shear shearing head and tail, pinch roll in front of laying machine, and laying into a loop , Air-cooled line to control cooling, volume and collection. The process is as follows:
(1)加热:采用步进梁式加热装置将截面尺寸为160mm×160mm的钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat a billet with a cross-sectional size of 160mm×160mm to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.346,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.233m/s,6V机架的出口速度为1.38m/s,经6道次轧制完成后轧件等效直径为75mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.346, and the deformation temperature is 850℃~1200℃. The exit speed of the 6V stand is 1.38m/s, and the equivalent diameter of the rolling stock is 75mm after 6 passes of rolling;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.289,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为1.38m/s,12V机架的出口速度为6.35m/s,经6道次轧制完成后轧件直径为35mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the head and tail of the flying shearing is subjected to 6 passes of rolling in the middle rolling mill, and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.289, the deformation temperature is 820 ° C ~ 1100 ° C, the bite of the 7H stand during the rolling process of the middle rolling mill The speed is 1.38m/s, the exit speed of the 12V stand is 6.35m/s, and the diameter of the rolled piece is 35mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)预精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次短应力线或悬臂轧机预精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.253,变形温度为800℃~1050℃,预精轧机组轧制过程中13H机架的咬入速度为6.35m/s,18V机架的出口速度为12.45m/s,经6道次轧制完成后轧件直径为25.0mm;(5) Pre-finishing rolling unit rolling: After controlling the cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 4 passes of short stress line or cantilever rolling mill pre-finishing rolling unit rolling , The pass system during rolling is an elliptical-circular pass system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.253, and the deformation temperature is 800℃~1050℃. During the rolling process of the rolling mill, the bite speed of the 13H stand is 6.35m/s, the exit speed of the 18V stand is 12.45m/s, and the diameter of the rolled piece after 6 passes of rolling is 25.0mm;
(6)预精轧后控制冷却:对步骤(5)经预精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50~200℃;(6) Controlled cooling after pre-finishing rolling: control water-cooling and recovery of the rolled piece after pre-finishing rolling in step (5), and the temperature drop range of a single water tank is 50-200°C;
(7)精轧后控制冷却:对步骤(6)经精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(7) Controlled cooling after finishing rolling: the rolling stock after finishing rolling in step (6) is subjected to controlled water cooling and recovery, and the temperature drop range of a single water tank is 50°C to 200°C;
(8)减定径机组轧制:对步骤(7)经精轧后控制冷却的轧件进行4道次45°顶交悬臂减定径机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.111,变形温度为850℃~990℃,减定径机组轧制过程中27#机架的咬入速度为12.45m/s,30#机架的出口速度为18.9m/s,经4道次轧制完成后轧件直径为20.0mm;(8) Rolling by reducing and sizing unit: 4 passes of 45° top-cross cantilever reducing and sizing unit rolling is performed on the rolled piece that has been controlled and cooled after finishing rolling in step (7), and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.111, and the deformation temperature is 850 ℃ ~ 990 ℃. The bite speed is 12.45m/s, the exit speed of the 30# stand is 18.9m/s, and the diameter of the rolled piece after 4 passes of rolling is 20.0mm;
(9)减定径后控制冷却:对步骤(8)经减定径轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(9) Controlled cooling after reducing and sizing: The rolling stock after reducing and sizing rolling in step (8) is controlled for water cooling and recovery, and the temperature drop range of a single water tank is 50°C to 200°C;
(10)吐丝、风冷线控制冷却及收集:对步骤(9)经减定径后控制冷却的轧件进行夹送吐丝,吐丝温度为800℃~1000℃,吐丝后进行风冷线控制冷却,不同钢种控制冷却工艺不同,风冷线的平均冷却速度范围为0.1℃/s~30℃/s,经风冷线控制冷却后轧件进行集卷,集卷温度范围为400℃~550℃,集卷后进行PF线冷却,经打包后称重收集。(10) Controlled cooling and collection of wire laying and air-cooling lines: pinch and lay the rolled piece that has been controlled and cooled after reducing and sizing in step (9). The cooling line is controlled for cooling. Different steel grades control the cooling process differently. The average cooling rate of the air-cooled line ranges from 0.1℃/s to 30℃/s. 400 ℃ ~ 550 ℃, PF line cooling after collection, weighing and collecting after packaging.
实施例6——大盘卷Example 6 - Large Coil
表2大盘卷各规格轧制速度及小时产量Table 2 Rolling speed and hourly output of each specification of large coil
参照图1、图5、图7与表2,按照本发明,生产工艺顺序包括:加热装置加热、粗轧机组轧制、粗轧后飞剪切头尾、中轧机组轧制、中轧后水冷及回复、中轧后飞剪切头尾、精轧机组轧制、精轧后水冷及回复、减定径前飞剪切头尾、三辊式减定径机组轧制、减定径后水冷及回复、卷取机卷曲、集卷及收集。该工艺具体如下:Referring to Fig. 1, Fig. 5, Fig. 7 and Table 2, according to the present invention, the production process sequence includes: heating by heating device, rolling in rough rolling group, flying shearing head and tail after rough rolling, rolling in intermediate rolling group, after intermediate rolling Water cooling and recovery, flying shearing head and tail after intermediate rolling, rolling in finishing mill, water cooling and recovery after finishing rolling, flying shearing head and tail before reducing and sizing, rolling in three-roll reducing and sizing unit, after reducing and sizing Water cooling and recovery, coiler coiling, coiling and collecting. The process is as follows:
(1)加热:采用步进梁式加热装置将截面尺寸为200mm×200mm的钢坯加热到900℃~1300℃;(1) Heating: use a walking beam heating device to heat a billet with a cross-sectional size of 200mm×200mm to 900℃~1300℃;
(2)粗轧机组轧制:采用平立交替的方式对步骤(1)加热后的方坯进行6道次短应力线粗轧机组轧制,粗轧机组轧制时,可采用无孔型轧制及孔型轧制,采用孔型轧制时,粗轧机组为箱型-箱型-椭圆-圆孔型系统,采用孔型轧制时每一架轧机前后均设有导卫,粗轧机组后设有飞剪,轧制过程中道次变形平均延伸率为1.296,变形温度为850℃~1200℃,粗轧机组轧制过程中1H机架的咬入速度为0.147m/s,6V机架的出口速度为0.70m/s,经6道次轧制完成后轧件等效直径为105mm;(2) Rough rolling mill rolling: The billet heated in step (1) is subjected to 6-pass short stress line rough rolling mill rolling in a horizontal and vertical alternate manner. During rough rolling mill rolling, no-pass type can be used. Rolling and pass rolling, when pass rolling is used, the rough rolling unit is a box-box-ellipse-round pass system. There is a flying shear behind the rolling mill. During the rolling process, the average elongation of the pass deformation is 1.296, and the deformation temperature is 850 ° C ~ 1200 ° C. The exit speed of the 6V stand is 0.70m/s, and the equivalent diameter of the rolled piece after 6 passes of rolling is 105mm;
(3)中轧机组轧制:对步骤(2)经粗轧后,并经飞剪切头尾后的轧件进行6道次中轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.281,变形温度为820℃~1100℃,中轧机组轧制过程中7H机架的咬入速度为0.70m/s,12V机架的出口速度为3.08m/s,经6道次轧制完成后轧件直径为50mm;(3) Rolling in the middle rolling mill: After rough rolling in step (2), the rolling stock after the head and tail of the flying shearing is subjected to 6 passes of rolling in the middle rolling mill, and the pass system during rolling is ellipse-circle Pass system, there are guides before and after each rolling mill, the average elongation of the pass deformation during the rolling process is 1.281, and the deformation temperature is 820℃~1100℃. The speed is 0.70m/s, the exit speed of the 12V stand is 3.08m/s, and the diameter of the rolled piece is 50mm after 6 passes of rolling;
(4)中轧后控制冷却:对步骤(3)经中轧后的轧件进行控制水冷并回复,单个水箱的温降范围为30℃~150℃;(4) Controlled cooling after intermediate rolling: control water cooling and recovery of the rolled piece after intermediate rolling in step (3), and the temperature drop range of a single water tank is 30°C to 150°C;
(5)精轧机组轧制:对步骤(4)经中轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次短应力线精轧机组轧制,轧制时孔型系统为椭圆-圆孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.250,变形温度为800℃~1050℃,精轧机组轧制过程中13H机架的咬入速度为3.08m/s,18V机架的出口速度为7.52m/s,经4道次轧制完成后轧件直径为32mm;(5) Finishing rolling mill rolling: After controlling cooling after intermediate rolling in step (4), the rolling stock after flying shearing head and tail is subjected to 4-pass short stress line finishing rolling mill rolling. The forming system is an ellipse-circular pass type system. There are guides before and after each rolling mill. During the rolling process, the average elongation of the pass deformation is 1.250, and the deformation temperature is 800 ° C ~ 1050 ° C. During the rolling process of the finishing rolling unit The bite speed of the 13H stand is 3.08m/s, the exit speed of the 18V stand is 7.52m/s, and the diameter of the rolled piece is 32mm after 4 passes of rolling;
(6)精轧后控制冷却:对步骤(5)经精轧轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(6) Controlled cooling after finishing rolling: The rolling stock after finishing rolling in step (5) is controlled by water cooling and recovered, and the temperature drop range of a single water tank is 50°C to 200°C;
(7)减定径机组轧制:对步骤(6)经精轧后控制冷却后,并经飞剪切头尾后的轧件进行4道次减定径机组轧制,轧制时孔型系统为弧三角-弧三角-弧三角-弧三角孔型系统,每一架轧机前后均设有导卫,轧制过程中道次变形平均延伸率为1.124,变形温度为750℃~950℃,减定径机组轧制过程中19#机架的咬入速度为7.52m/s,22#机架的出口速度为12.01m/s,经4道次轧制完成后轧件直径为25.0mm;(7) Rolling by reducing and sizing unit: After controlling the cooling after finishing rolling in step (6), the rolling stock after the head and tail of flying shearing is subjected to 4 passes of reducing and sizing unit rolling. The system is arc-triangle-arc-triangle-arc-triangle-arc-triangle pass system. Guide guards are provided before and after each rolling mill. During the rolling process, the average elongation of pass deformation is 1.124, and the deformation temperature is 750℃~950℃. During the rolling process of the reducing and sizing unit, the bite speed of the 19# stand is 7.52m/s, the exit speed of the 22# stand is 12.01m/s, and the diameter of the rolled piece after 4 passes of rolling is 25.0mm;
(8)减定径后控制冷却:对步骤(7)经减定径轧制后的轧件进行控制水冷并回复,单个水箱的温降范围为50℃~200℃;(8) Controlled cooling after reducing and sizing: The rolling stock after reducing and sizing rolling in step (7) is controlled by water cooling and recovered, and the temperature drop range of a single water tank is 50°C to 200°C;
(9)卷取机卷曲、收集:对步骤(8)经减定径后控制冷却的轧件进行卷曲,卷曲温度为700℃~1000℃,卷曲后进行PF线冷却,经打包后称重收集。(9) Coiler coiling and collection: coil the rolled piece that has been controlled and cooled after reducing and sizing in step (8), and the coiling temperature is 700 ° C ~ 1000 ° C. After coiling, PF line cooling is performed, and after packaging, weighing and collection .
最后说明的是,以上实施例仅用以说明本发明的技术方案而非限制,尽管参照较佳实施例对本发明进行了详细说明,本领域的普通技术人员应当理解,可以对本发明的技术方案进行修改或者等同替换,而不脱离本技术方案的宗旨和范围,其均应涵盖在本发明的权利要求范围当中。Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to the preferred embodiments, those of ordinary skill in the art should understand that the technical solutions of the present invention can be Modifications or equivalent replacements, without departing from the spirit and scope of the technical solution, should all be included in the scope of the claims of the present invention.
Claims (10)