CN114142105B - Winding battery core, preparation method thereof and winding battery - Google Patents
Winding battery core, preparation method thereof and winding battery Download PDFInfo
- Publication number
- CN114142105B CN114142105B CN202111210302.8A CN202111210302A CN114142105B CN 114142105 B CN114142105 B CN 114142105B CN 202111210302 A CN202111210302 A CN 202111210302A CN 114142105 B CN114142105 B CN 114142105B
- Authority
- CN
- China
- Prior art keywords
- area
- blank area
- sheet
- width
- winding
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The invention discloses a preparation method of a winding battery, which comprises the following steps: (1) Providing an aluminum foil, coating positive electrode slurry on the front and back surfaces of the aluminum foil, and connecting a first tab to obtain a cathode sheet, wherein the first tab is arranged between a winding starting end and a winding tail end of the cathode sheet; (2) Providing copper foil, coating negative electrode slurry on the front and back surfaces of the copper foil, and bonding second lugs to obtain an anode sheet, wherein the second lugs are arranged between the winding starting end and the winding tail end of the anode sheet; (3) providing a membrane sheet; (4) And sequentially laminating and winding the anode sheet, the diaphragm sheet and the cathode sheet to form a winding battery cell. The invention also provides a winding battery core prepared by the method, and a winding battery prepared by the technical scheme. According to the invention, the positions of the tabs and the winding mode of the wound battery are changed, so that the area of a blank area can be reduced by the anode sheet, the load capacity of the cathode slurry is increased, and the battery capacity is further increased.
Description
Technical Field
The invention relates to the technical field of lithium batteries, in particular to a winding battery core, a preparation method thereof and a winding battery.
Background
A battery composed of cells formed by winding is called a wound battery. The winding battery has super-strong high-rate discharge capacity, and the maximum discharge rate is 18C10; excellent high and low temperature performance, and can work at-55-75 ℃; smooth high output voltage, higher energy density; the structure is firm, and the shock resistance is excellent; free electrolyte is not provided, and the electrolyte can be placed in any direction for working; the quick charging can be carried out, and more than 95% of electric quantity can be charged within 40 minutes; the super-long life, the designed floating charge life can reach more than 8 years; extremely high small current deep discharge resistance. The coiled battery has the advantages that the coiled battery is suitable for the field of new energy automobiles, but with the rapid development of the new energy automobile industry, the energy density requirement on the power battery is higher and higher.
In the traditional winding battery, due to the arrangement mode and the winding mode of the lugs, a large area of the anode sheet which is not coated with plasma materials is reserved, so that the materials of the anode sheet of the winding battery are wasted, and the energy density of the winding battery is limited.
Disclosure of Invention
The invention aims to overcome the defects of the prior art, and provides a preparation method of a winding electric core, which can improve the electrode slurry loading capacity of the winding electric core.
The invention also provides a winding cell with higher electrode slurry loading capacity.
The invention also provides a winding battery with higher battery energy density.
In order to solve the above problems, the present invention provides a method for manufacturing a wound cell, comprising:
(1) Providing an aluminum foil, coating positive electrode slurry on the front and back surfaces of the aluminum foil, and connecting a first tab to obtain a negative electrode plate; the front surface of the cathode sheet is provided with a first positive electrode slurry coating area and a first blank area; the back of the cathode sheet is provided with a second anode slurry coating area and a second blank area; the first blank area and the second blank area are arranged at the winding tail end of the cathode sheet; the first positive electrode slurry coating area is provided with a third blank area, the third blank area is arranged between the winding starting end and the winding tail end, and the first tab is connected with the third blank area;
(2) Providing copper foil, coating negative electrode slurry on the front and back surfaces of the copper foil, and bonding second lugs to obtain an anode plate; the front surface of the anode sheet is provided with a first negative electrode slurry coating area and a fourth blank area; the back of the anode sheet is provided with a second anode slurry coating area and a fifth blank area; the fourth blank area and the fifth blank area are arranged at the winding tail end of the anode sheet; the first negative electrode slurry coating area is provided with a sixth blank area, the sixth blank area is far away from the winding starting end of the anode sheet, and the second lug is connected with the sixth blank area;
(3) Providing a diaphragm;
(4) And sequentially laminating and winding the anode sheet, the diaphragm sheet and the cathode sheet to form a winding battery cell.
As an improvement of the above technical solution, the first positive electrode slurry coating area is further provided with a seventh blank area, and the seventh blank area is disposed in a folded angle of the winding start end of the cathode sheet.
As an improvement of the technical scheme, the width of the seventh blank area is the same as the width of the aluminum foil, and the length of the seventh blank area is 1-3 mm.
As an improvement of the technical scheme, the widths of the first blank-keeping area and the second blank-keeping area are the same as the width of the aluminum foil, and the lengths of the first blank-keeping area and the second blank-keeping area are 25-35 mm;
The width of the fourth blank area and the width of the fifth blank area are the same as the width of the copper foil, and the length of the fourth blank area and the fifth blank area is 25-35 mm.
As an improvement of the technical scheme, the first positive electrode slurry coating area and the first negative electrode slurry coating area are respectively provided with through holes, the distance between every two adjacent through holes is 2-3 mm, and the aperture of each through hole is smaller than 1mm.
As an improvement of the above technical scheme, the preparation method of the cathode sheet provided with the through hole comprises the following steps:
(1.1) providing an aluminum foil, and forming a through hole area on the surface of the aluminum foil, wherein the length of the through hole area is the same as that of the aluminum foil, and the width of the through hole area is smaller than that of the aluminum foil, so that blank areas with the width of 20-30 mm are reserved on two sides of the aluminum foil;
(1.2) coating positive electrode slurry on the through hole areas on the front and back surfaces of the aluminum foil, cutting a blank area after coating, and connecting a first tab after cutting to obtain a cathode sheet;
the preparation method of the anode sheet provided with the through holes comprises the following steps:
(2.1) providing a copper foil, and forming a through hole region on the surface of the copper foil, wherein the length of the through hole region is the same as that of the copper foil, and the width of the through hole region is smaller than that of the copper foil, so that blank regions with the width of 20-30 mm are reserved on two sides of the copper foil;
And (2.2) coating the cathode slurry on the through hole areas on the front and back surfaces of the copper foil, cutting the blank area after coating, and connecting the second electrode tab to the anode sheet after cutting.
As an improvement of the above technical scheme, the width of the first positive electrode slurry coating area is 60-70 mm, and the width of the first negative electrode slurry coating area is 60-70 mm.
As an improvement of the above technical solution, the width of the third blank area is smaller than the width of the aluminum foil.
Correspondingly, the invention also provides a winding battery cell, which is prepared by the preparation method of the winding battery cell.
Correspondingly, the invention also provides a winding battery which comprises the winding battery core.
The implementation of the invention has the following beneficial effects:
The invention provides a preparation method of a winding battery core, which is characterized in that the arrangement position of a tab is moved from a winding starting end to a winding starting end far away from a pole piece, and the winding mode between an anode sheet and a cathode sheet is improved, so that the area of a blank area can be reduced by the anode sheet, more electrode slurry can be loaded on the winding battery core, and the energy density of a battery is increased.
The invention also provides a winding battery cell which is prepared by the preparation method of the battery cell, and compared with the traditional preparation method of the winding battery cell, the prepared battery cell has higher electrode slurry loading capacity.
The invention also provides a winding battery which contains the battery core and has higher battery capacity than a battery with the same volume.
Drawings
In order to more clearly illustrate the embodiments of the invention or the technical solutions in the prior art, the drawings that are required in the embodiments or the description of the prior art will be briefly described, it being obvious that the drawings in the following description are only some embodiments of the invention, and that other drawings may be obtained according to these drawings without inventive effort for a person skilled in the art.
FIG. 1 is a flow chart of the present invention for preparing a wound cell;
FIG. 2 is a schematic view of a wound cell made in accordance with the present invention;
FIG. 3 is a schematic front view of a cathode sheet of the present invention;
FIG. 4 is a schematic rear view of a cathode sheet of the present invention;
FIG. 5 is a schematic front view of an anode sheet of the present invention;
FIG. 6 is a schematic rear view of an anode sheet of the present invention;
FIG. 7 is a schematic front view of the present invention with the original aluminum foil perforated and not cut;
FIG. 8 is a schematic front view of a cathode sheet provided with a through hole according to the present invention;
FIG. 9 is a schematic front view of the original copper foil of the present invention after punching, without cutting;
FIG. 10 is a schematic front view of an anode sheet provided with through holes according to the present invention;
fig. 11 is a schematic diagram of the stacking of the cathode sheet, anode sheet and separator sheet during winding of the present invention.
Detailed Description
The following description of the embodiments of the present invention will be made clearly and completely with reference to the accompanying drawings, in which it is apparent that the embodiments described are only some embodiments of the present invention, but not all embodiments. All other embodiments, which can be made by those skilled in the art based on the embodiments of the invention without making any inventive effort, are intended to be within the scope of the invention.
Referring to fig. 1, the invention provides a preparation method of a winding cell, comprising the following steps:
S1: providing an aluminum foil 11, coating positive electrode slurry on the front and back surfaces of the aluminum foil, and connecting a first tab 13 to obtain a cathode sheet 1;
Referring to fig. 3 and 4, the front surface of the cathode sheet is provided with a first positive electrode slurry coating region 12 and a first blank region 14, and the back surface of the cathode sheet 1 is provided with a second positive electrode slurry coating region 16 and a second blank region 15. The first and second blank areas 14 and 15 are provided at the winding end of the cathode sheet 1.
The widths of the first blank area 14 and the second blank area 15 are 60-70 mm, which is the same as the width of the aluminum foil 11. The first and second blank areas 14,15 are the same in length, 25 to 35mm, and exemplary 26mm, 29mm, 32mm, 35mm, but are not limited thereto. The first blank area 14 and the second blank area 15 are used for pasting green glue after winding is finished, and the green glue is used for fixing the winding battery cell.
Wherein the first and second positive electrode slurry coating regions 12 and 16 have the same width. In one embodiment of the present invention, the width of both is 60 to 70mm, which is the same as the width of the aluminum foil 1. In another embodiment of the present invention, through holes 4 are provided on the first positive electrode slurry coating 12, and the distance between adjacent through holes 4 is 2 to 3mm, and exemplary are 2mm, 2.4mm, 2.8mm, 3mm, but not limited thereto. When the distance between the through holes is less than 2mm, the number of through holes in the aluminum foil 11 is excessive, and the aluminum foil is easily broken. When the distance between the adjacent through holes 4 is more than 3mm, the number of the through holes on the aluminum foil 1 is too small, and the effect of increasing the anode slurry load is not achieved. The diameter of the through hole 4 is < 1mm, and exemplary examples are, but not limited to, 0.5mm, 0.7mm, 0.8mm, and 0.9mm (see fig. 8).
Specifically, the preparation method of the cathode plate provided with the through hole comprises the following steps:
(1.1): providing an aluminum foil, and forming a through hole area on the surface of the aluminum foil, wherein the length of the through hole area is the same as that of the aluminum foil, and the width of the through hole area is smaller than that of the aluminum foil, so that blank areas with the width of 20-30 mm are reserved on two sides of the aluminum foil (see FIG. 7);
The widths of the blank areas are exemplified by, but not limited to, 20, 24, 27, and 30mm, and the blank areas 122 are provided at the top and the top of the through-hole area of the aluminum foil in order to ensure the structural strength of the original copper foil, so that the original aluminum foil is not easily broken when the electrode paste is coated in the next step.
(1.2): Coating positive electrode slurry on the through hole areas of the front and back surfaces of the original aluminum foil, cutting the blank area 122 after coating, and connecting the cut blank area to the cathode sheet 11 of the first tab 13 (see fig. 8);
The first positive electrode slurry coating area 12 and/or the second positive electrode slurry coating area 16 are/is provided with a third blank area 18, the third blank area 18 is arranged between the winding start end and the winding tail end, and the first tab 13 is connected with the third blank area 18.
Preferably, the third blank 18 is disposed on the first positive electrode slurry coating zone 12. Referring to fig. 3, the first positive electrode slurry coating zone 12 includes a plurality of cathode folded sections 121 distributed along the cathode sheet 1, and the third blank 18 is disposed on the 4 th, 6 th and/or 8 th positive electrode slurry coating sections from the winding start of the cathode sheet 1. Specifically, the width of the third blank 18 is smaller than the width of the aluminum foil 11 so that the aluminum foil 11 is loaded with more positive electrode slurry.
Preferably, the first positive electrode slurry coating region 12 is further provided with a seventh blank 17, and the seventh blank 17 is provided inside the fold angle of the winding start end of the cathode sheet 1, that is, between the 1 st cathode folded section 121a and the second cathode folded section 121b (see fig. 3). The angle of the folding angle of the winding starting end of the cathode plate 1 is larger, and the seventh white-keeping area 17 is arranged, so that the positive electrode slurry can be effectively prevented from falling off. Specifically, the seventh blank 17 has the same width as the aluminum foil 11 and a length of 1 to 3mm. Exemplary are, but not limited to, 1.5mm, 1.8mm, 2.3mm, 2.7 mm.
S2: providing a copper foil 21, coating negative electrode slurry on the front and back surfaces of the copper foil, and bonding a second tab 23 to obtain an anode sheet 2;
Referring to fig. 5 and 6, the front surface of the anode sheet 2 is provided with a first anode slurry coating region 22 and a first blank region 24, and the back surface of the anode sheet 2 is provided with a second anode slurry coating region 26 and a second blank region 25. The fourth blank 24 and the fifth blank 25 are provided at the winding end of the anode sheet 2.
The width of the fourth and fifth blank areas 24, 25 is 60 to 70mm, which is the same as the width of the copper foil 21. The fourth and fifth blank areas 24, 25 are the same in length, 25 to 35mm, and exemplary 26mm, 29mm, 32mm, 35mm, but are not limited thereto. The fourth blank area 24 and the fifth blank area 25 are used for pasting green glue after winding is finished, and the green glue is used for fixing the winding cell.
Wherein the widths of the first and second anode slurry coating regions 22 and 26 are the same. In one embodiment of the present invention, the width of both is 60 to 70mm, which is the same as the width of the copper foil 1. In another embodiment of the present invention, through holes 4 are provided on the first negative electrode slurry coating region 22, and the distance between adjacent through holes 4 is 2 to 3mm, and exemplary are 2mm, 2.4mm, 2.8mm, and 3mm, but not limited thereto.
Specifically, the preparation method of the anode sheet provided with the through holes comprises the following steps:
(2.1): providing a copper foil, and forming a through hole region on the surface of the copper foil, wherein the length of the through hole region is the same as that of the copper foil, and the width of the through hole region is smaller than that of the copper foil, so that blank regions with the width of 20-30 mm are reserved on two sides of the copper foil (see FIG. 9);
the first anode slurry coating area 22 and/or the second anode slurry coating area 26 are/is provided with a sixth blank area 27, the sixth blank area 27 is disposed away from the winding start end of the anode sheet 2, and the second tab 23 is connected with the sixth blank area 27.
(2.2): The cathode paste is coated on the through hole regions of the front and back surfaces of the original copper foil, the blank region 122 is cut after the coating, and the second tab 23 is connected to the anode sheet after the cutting (see fig. 10).
Wherein a sixth blank area 27 is provided on the first anode slurry coating area 22. Referring to fig. 3, the first anode slurry coating zone 22 includes a plurality of anode folding sections distributed along the anode sheet 2, and a sixth blank area 27 is provided on the 4 th, 6 th and/or 8 th anode slurry coating sections from the winding start of the anode sheet 2.
Referring to fig. 3, the width of the sixth blank area 27 is smaller than the width of the copper foil 21 so that the copper foil 21 is loaded with more positive electrode paste.
S3: providing a diaphragm 3;
Specifically, the length of the diaphragm sheet 3 is twice or more the length of the anode sheet 1.
S4: sequentially laminating and winding an anode sheet, a diaphragm sheet and a cathode sheet to form a winding battery cell;
Referring to fig. 11, in detail, the anode sheet 2 includes a plurality of anode folded sections, and the cathode sheet 1 includes a plurality of cathode folded sections.
The first step, the diaphragm 3 is folded in half along the length direction;
Secondly, placing the anode sheet 2 in the middle of the folded diaphragm sheet; the winding initial end of the anode sheet 2 is aligned with the folded position of the diaphragm sheet; obtaining a first intermediate;
And a third step of: folding the first intermediate in half along the first anode sheet folding section 27 of the anode sheet 2 to obtain a second intermediate;
fourth step: placing the cathode sheet 1 in the folded position of the second intermediate body, and aligning 18 the first anode sheet folding section 27 of the anode sheet 2 with the first cathode sheet folding section of the cathode sheet 1; obtaining a third intermediate;
fifth step: and sequentially laminating and winding the third intermediate to obtain the winding battery cell.
Example 1:
the embodiment provides a winding cell:
(1) Providing an aluminum foil with a width of 67mm, coating positive electrode slurry on the front and back surfaces of the aluminum foil, connecting the first tab to obtain a cathode sheet,
Wherein the positive electrode slurry was prepared by mixing 90wt% of lini0.5co0.2mn0.3o2, 5wt% of super P, 5wt% of pvdf, adding NMP solvent (60% of the sum of the mass of the first three substances), and stirring for 4 hours.
The front surface of the cathode plate is provided with a first positive electrode slurry coating area and a first blank area, and the back surface of the cathode plate is provided with a second positive electrode slurry coating area and a second blank area. The first and second blank areas are disposed at the winding end of the cathode sheet. The lengths of the first positive electrode slurry coating area and the second positive electrode slurry coating area are 1200mm; the length of the first blank area and the second blank area is 29mm;
The widths of the first blank area and the second blank area are the same as the width of the aluminum foil and are 67mm. The length of the first blank area and the second blank area are the same and are 29mm.
And the first positive electrode slurry coating area is provided with a third blank area, the third blank area is far away from the winding starting end of the cathode plate, and the first tab is connected with the third blank area.
Specifically, in one embodiment of the present invention, the first positive electrode slurry coating region 12 is further provided with a seventh blank 17, the seventh blank 17 being provided inside the folded angle of the winding start end of the cathode sheet 1, the seventh blank having a length of 2mm.
(2) A copper foil having a width of 69mm was provided, and the front and back sides of the copper foil were coated with a negative electrode paste and connected to a second tab to obtain an anode sheet.
The front surface of the anode sheet is provided with a first anode slurry coating area and a fourth blank area, and the back surface of the anode sheet is provided with a second anode slurry coating area and a fifth blank area. The fourth blank area and the fifth blank area are arranged at the winding tail end of the anode sheet, the length of the fourth blank area and the length of the fifth blank area are 29mm, and the width of the fourth blank area and the width of the fifth blank area are 69mm, which are the same as the width of the copper foil.
The first negative electrode slurry coating area and/or the second negative electrode slurry coating area are/is provided with a sixth blank area, the sixth blank area is far away from the winding starting end of the anode sheet, and the second lug is connected with the sixth blank area. In the present embodiment, a sixth blank region is provided on the first anode slurry coating region, the sixth blank region is provided at the 4 th from the starting end of the anode sheet winding, and the width of the sixth blank region is smaller than the width of the copper foil
Providing a diaphragm, wherein the length of the diaphragm is twice or more than that of the anode plate;
and sequentially laminating and winding the anode sheet, the diaphragm sheet and the cathode sheet to form a winding battery cell.
The wound battery made from the wound cell of example 1 had an energy density of 261.23wh/kg by an electrolyte voltage regulator.
Example 2:
the embodiment provides a winding cell:
example 2 differs from example 1 in that;
The first positive electrode slurry coating area of the negative electrode plate is provided with through holes with the aperture of 0.7mm and the distance between adjacent through holes of 2 mm; the first negative electrode slurry coating area of the anode sheet is provided with through holes with the aperture of 0.7mm and the distance between adjacent through holes of 2 mm.
The wound cell made from the wound cell of example 2 had an energy density of 289.97wh/kg by means of an electrowinning voltage regulator.
In addition, the wound battery provided by the embodiment of the present invention has been described in detail, and specific examples are applied herein to illustrate the principles and embodiments of the present invention, and the description of the above examples is only for helping to understand the method and core idea of the present invention; meanwhile, as those skilled in the art will have variations in the specific embodiments and application scope in accordance with the ideas of the present invention, the present description should not be construed as limiting the present invention in view of the above.
Claims (9)