CN111424163A - Equipment and process for quickly realizing temperature transition of strip steel in continuous annealing furnace - Google Patents

Equipment and process for quickly realizing temperature transition of strip steel in continuous annealing furnace Download PDF

Info

Publication number
CN111424163A
CN111424163A CN201910022891.3A CN201910022891A CN111424163A CN 111424163 A CN111424163 A CN 111424163A CN 201910022891 A CN201910022891 A CN 201910022891A CN 111424163 A CN111424163 A CN 111424163A
Authority
CN
China
Prior art keywords
heating
strip steel
temperature
section
magnetic induction
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910022891.3A
Other languages
Chinese (zh)
Inventor
胡广魁
陈云鹏
汤文杰
张理扬
袁俭
朱砚刚
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Baoshan Iron and Steel Co Ltd
Original Assignee
Baoshan Iron and Steel Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Baoshan Iron and Steel Co Ltd filed Critical Baoshan Iron and Steel Co Ltd
Priority to CN201910022891.3A priority Critical patent/CN111424163A/en
Publication of CN111424163A publication Critical patent/CN111424163A/en
Pending legal-status Critical Current

Abstract

本发明公开了一种连续退火炉内快速实现带钢温度过渡的设备及工艺,包括:依次连接的加热段、横磁感应加热、辐射管均热段、缓冷段和快冷段。所述的加热段为依次连接的直火加热段和辐射管加热段。所述的加热段为直火加热段。所述的加热段为纵磁感应加热。本发明通过快速调整加热设备的加热负荷,以期达到快速改变带钢温度,满足带钢规格变化或退火曲线变化时对带钢温度快速响应的需求。

Figure 201910022891

The invention discloses a device and a process for rapidly realizing temperature transition of strip steel in a continuous annealing furnace, comprising: a heating section, a transverse magnetic induction heating, a radiant tube soaking section, a slow cooling section and a fast cooling section connected in sequence. The heating section is a direct fire heating section and a radiant tube heating section which are connected in sequence. The heating section is a direct-fire heating section. The heating section is longitudinal magnetic induction heating. The invention quickly adjusts the heating load of the heating equipment, so as to achieve the rapid change of the strip steel temperature and meet the requirements of rapid response to the strip steel temperature when the strip steel specification changes or the annealing curve changes.

Figure 201910022891

Description

一种连续退火炉内快速实现带钢温度过渡的设备及工艺A kind of equipment and process for rapidly realizing strip temperature transition in continuous annealing furnace

技术领域technical field

本发明涉及钢带连续热处理领域,更具体地说,涉及一种连续退火炉内快速实现带钢温度过渡的设备及工艺。The invention relates to the field of continuous heat treatment of steel strips, in particular to a device and a process for rapidly realizing temperature transition of strip steel in a continuous annealing furnace.

背景技术Background technique

在连续退火炉内,冷轧后的带钢经过加热和冷却等各热处理工艺处理后,才能达到用户所需要的机械性能。传统连续退火炉如图1所示,主要包括加热段1、均热段2、缓冷段3、快冷段4等工艺段,带钢5先后经过各工艺段完成热处理过程。热处理工艺包含各工艺温度的检测、工艺温度控制以及热处理时间控制。其中,工艺温度控制主要包括加热温度控制和冷却温度控制。加热温度的控制一般通过直火加热、燃气辐射管加热、电加热、感应加热等加热方式实现,冷却温度的控制一般通过喷气冷却、水冷辊冷却、水淬冷却等方式实现。以常用的喷气冷却方式而言,冷却温度的调节是通过改变冷却风机的转速达到温度的快速切换的目的。但相对于冷却温度的控制,由于加热造成炉膛的热惯性很强,使得常规加热方式所能实现的加热温度的调节控制反应速度远远低于冷却温度调节速度,造成在退火温度或带钢规格切换时容易造成实际带钢加热温度偏离控制目标,结果造成带钢性能不符。因此,有必要寻求一种能够实现加热温度快速切换的方式,大幅度减小退火温度或带钢规格过渡时造成的加热温度不符。In the continuous annealing furnace, the cold-rolled strip can only achieve the mechanical properties required by users after various heat treatment processes such as heating and cooling. As shown in Figure 1, the traditional continuous annealing furnace mainly includes heating section 1, soaking section 2, slow cooling section 3, fast cooling section 4 and other process sections. The heat treatment process includes the detection of each process temperature, the control of the process temperature and the control of the heat treatment time. Among them, the process temperature control mainly includes heating temperature control and cooling temperature control. The control of heating temperature is generally realized by heating methods such as direct fire heating, gas radiant tube heating, electric heating, and induction heating. In the common jet cooling method, the adjustment of the cooling temperature is to achieve the purpose of rapid temperature switching by changing the speed of the cooling fan. However, compared with the control of the cooling temperature, the thermal inertia of the furnace is very strong due to the heating, so that the adjustment and control reaction speed of the heating temperature that can be realized by the conventional heating method is far lower than the adjustment speed of the cooling temperature, resulting in the annealing temperature or strip specification. When switching, it is easy to cause the actual strip heating temperature to deviate from the control target, resulting in inconsistent strip performance. Therefore, it is necessary to find a way to achieve rapid switching of heating temperature, and greatly reduce the heating temperature difference caused by annealing temperature or strip specification transition.

在现有的连续退火炉中,带钢最高加热温度高达900℃,主要采用如图1的辐射管加热方式,平均加热速度一般在3-15℃/s内,带钢温度越高加热速度越慢。在实际生产中经常存在带钢规格和退火温度变化,需要降温时,由于加热炉的惯性大,降温速度慢;需要升温时,由于辐射管相对加热速度较慢,造成带钢升温速度慢。升降温都会造成温度过渡段很长且带钢温度不符,进而造成带钢性能不符。为解决此问题,实际生产中一般采用在成品生产计划中插入过渡用钢卷(非成品),这一方面占用了生产线的产能,还消耗了大量不必要的能源介质,因此有必要提高连续退火炉内带钢温度过渡的响应速度,减少过渡卷的使用,提高生产效率和改进产品质量。In the existing continuous annealing furnace, the maximum heating temperature of the strip is as high as 900 °C. The radiant tube heating method as shown in Figure 1 is mainly used. The average heating speed is generally within 3-15 °C/s. The higher the strip temperature, the faster the heating speed. slow. In actual production, there are often changes in strip specifications and annealing temperature. When cooling is required, the cooling rate is slow due to the large inertia of the heating furnace; when heating is required, the heating rate of the strip is slow due to the relatively slow heating rate of the radiant tube. The temperature rise and fall will cause the temperature transition section to be very long and the strip temperature to be inconsistent, thereby causing the strip performance to be inconsistent. In order to solve this problem, in actual production, it is generally used to insert transitional steel coils (non-finished products) in the finished product production plan, which occupies the production capacity of the production line and consumes a lot of unnecessary energy media, so it is necessary to improve the continuous return. The speed of response to the temperature transition of the strip in the furnace reduces the use of transition coils, increases production efficiency and improves product quality.

目前,国内外在连续退火炉内使用的加热技术有:直火加热、燃气辐射管加热、电加热、感应加热等,加热速度由快到慢的顺序是:感应加热>直火加热>燃气辐射管加热>电加热,炉膛热惯性由大到小的排序是:燃气辐射管加热>电加热>直火加热>感应加热,由以上分析可知,采用直火加热和感应加热既能够获取快的加热速度又能够同时具备热惯性小的优点,可以在实际连续退火生产中实现带钢温度的快速切换。这其中感应加热表现更加优异,但连续退火炉中一般使用的常规感应加热器都是纵磁感应加热(磁力线平行带钢),这种类型的感应加热器不能在700℃以上有效加热薄带钢,只有业界最新开发成功的横磁感应加热(磁力线垂直带钢)设备才能够有效实现700℃以上温度薄带钢的有效加热。关于横磁感应加热(磁力线垂直带钢)技术,目前全球范围内已经有法国FIVES集团下属的Cellas公司和比利时的Inducthern公司能够制造设备并已有使用实绩。At present, the heating technologies used in continuous annealing furnaces at home and abroad include: direct fire heating, gas radiant tube heating, electric heating, induction heating, etc. The order of heating speed from fast to slow is: induction heating > direct fire heating > gas radiation Tube heating > electric heating, the order of furnace thermal inertia from large to small is: gas radiant tube heating > electric heating > direct fire heating > induction heating. From the above analysis, it can be seen that the use of direct fire heating and induction heating can obtain fast heating. The speed can also have the advantage of small thermal inertia at the same time, which can realize rapid switching of strip temperature in actual continuous annealing production. Among them, the induction heating performance is more excellent, but the conventional induction heaters generally used in continuous annealing furnaces are longitudinal magnetic induction heating (magnetic lines of force parallel to the strip), this type of induction heater cannot effectively heat the thin strip above 700 ℃, Only the newly developed transverse magnetic induction heating (magnetic line vertical strip) equipment in the industry can effectively achieve the effective heating of thin strips with temperatures above 700 °C. Regarding the transverse magnetic induction heating (magnetic field line vertical strip) technology, there are already cellas company under the French FIVES group and the Belgian Inducthern company able to manufacture equipment and have already used it in the world.

以上述分析和描述的加热和冷却方式为基础,存在有开发出一种可以实现连续退火炉内带钢温度快速切换的控制模式的可能性,但实际工业化的使用实绩中没有发现类似的连续退火温度快速过渡控制技术,分析主要原因应该有以下几点:Based on the above analysis and description of the heating and cooling methods, it is possible to develop a control mode that can realize rapid switching of the strip temperature in the continuous annealing furnace, but no similar continuous annealing has been found in actual industrial use. The main reasons for the analysis of the rapid temperature transition control technology should be as follows:

1)之前感应加热设备制造厂家还没有开发出横磁感应加热设备,无法实现700℃以上碳钢薄带钢的加热;1) Before induction heating equipment manufacturers have not developed transverse magnetic induction heating equipment, they cannot achieve heating of carbon steel thin strips above 700 °C;

2)先进直火加热等技术还没有得到工业化的充分推广使用。2) Advanced direct fire heating and other technologies have not been fully promoted and used in industrialization.

发明内容SUMMARY OF THE INVENTION

针对现有技术中存在的上述缺陷,本发明的目的是提供一种连续退火炉内快速实现带钢温度过渡的设备及工艺,通过快速调整加热设备的加热负荷,以期达到快速改变带钢温度,满足带钢规格变化或退火曲线变化时对带钢温度快速响应的需求。In view of the above-mentioned defects existing in the prior art, the purpose of the present invention is to provide a device and process for rapidly realizing the temperature transition of the strip in a continuous annealing furnace. Meets the need for rapid response to strip temperature when strip specifications change or annealing curves change.

为实现上述目的,本发明采用如下技术方案:To achieve the above object, the present invention adopts the following technical solutions:

一方面,一种连续退火炉内快速实现带钢温度过渡的设备,包括:依次连接的加热段、横磁感应加热、辐射管均热段、缓冷段和快冷段,带钢依次输送通过加热段、横磁感应加热、辐射管均热段、缓冷段和快冷段。On the one hand, a device for rapidly realizing the temperature transition of strip steel in a continuous annealing furnace includes: a heating section, a transverse magnetic induction heating, a radiant tube soaking section, a slow cooling section and a fast cooling section connected in sequence, and the strip steel is transported in sequence through the heating section. section, transverse magnetic induction heating, radiant tube soaking section, slow cooling section and fast cooling section.

所述的加热段为依次连接的直火加热段和辐射管加热段。The heating section is a direct fire heating section and a radiant tube heating section which are connected in sequence.

所述的加热段为直火加热段。The heating section is a direct-fire heating section.

所述的加热段为纵磁感应加热。The heating section is longitudinal magnetic induction heating.

另一方面,一种连续退火炉内快速实现带钢温度过渡的工艺:On the other hand, a process for rapidly realizing strip temperature transition in a continuous annealing furnace:

当带钢温度小于600℃时,采用辐射管加热段进行加热,当带钢温度大于600℃时,采用横磁感应加热将带钢加热至目标温度,当带钢的规格或退火曲线发生变化时,通过横磁感应加热的加热功率调整带钢的温度;When the strip temperature is less than 600°C, the heating section of the radiant tube is used for heating. When the strip temperature is greater than 600°C, the strip is heated to the target temperature by transverse magnetic induction heating. When the strip specification or annealing curve changes, Adjust the temperature of the strip through the heating power of the transverse magnetic induction heating;

当带钢温度小于600℃时,采用直火加热段进行加热,当带钢温度大于600℃时,采用辐射管加热段继续将带钢加热到700℃以下,当带钢温度达到700℃以上时,采用横磁感应加热将带钢加热至目标温度,当带钢的规格或退火曲线发生变化时,通过直火加热段的燃烧负荷和横磁感应加热的加热功率调整带钢的温度;When the temperature of the strip steel is less than 600℃, use the direct fire heating section for heating. When the temperature of the strip steel is greater than 600℃, use the radiant tube heating section to continue heating the steel strip to below 700℃. When the temperature of the strip steel reaches above 700℃ , using transverse magnetic induction heating to heat the strip to the target temperature, when the specification of the strip or the annealing curve changes, the temperature of the strip is adjusted by the combustion load of the direct fire heating section and the heating power of the transverse magnetic induction heating;

当带钢温度小于700℃时,采用直火加热段进行加热,当带钢温度达到700℃以上时,采用横磁感应加热将带钢加热至目标温度,当带钢的规格或退火曲线发生变化时,通过直火加热段的燃烧负荷和横磁感应加热的加热功率调整带钢的温度;When the temperature of the strip steel is less than 700℃, the direct heating section is used for heating. When the temperature of the strip steel reaches above 700℃, the transverse magnetic induction heating is used to heat the strip steel to the target temperature. When the specifications of the strip steel or the annealing curve change , adjust the temperature of the strip through the combustion load of the direct fire heating section and the heating power of the transverse magnetic induction heating;

利用纵磁感应加热将带钢加热至700℃,当带钢温度达到700℃以上时,采用横磁感应加热将带钢加热至目标温度,当带钢的规格或退火曲线发生变化时,通过纵磁感应加热的加热功率和横磁感应加热的加热功率调整带钢的温度。Use longitudinal magnetic induction heating to heat the strip to 700°C. When the temperature of the strip reaches above 700°C, use transverse magnetic induction heating to heat the strip to the target temperature. When the specification or annealing curve of the strip changes, the longitudinal magnetic induction heating is used. The heating power and the heating power of the transverse magnetic induction heating adjust the temperature of the strip.

所述的辐射管加热段的加热速度为20-30℃/s,横磁感应加热的加热速度为100-300℃/s,直火加热段的加热速度为50-100℃/s,纵磁感应加热的加热速度为100-300℃/s。The heating speed of the heating section of the radiant tube is 20-30 °C/s, the heating speed of the transverse magnetic induction heating is 100-300 °C/s, the heating speed of the direct fire heating section is 50-100 °C/s, and the heating speed of the longitudinal magnetic induction heating is 50-100 °C/s. The heating rate is 100-300℃/s.

在上述的技术方案中,本发明所提供的一种连续退火炉内快速实现带钢温度过渡的设备及工艺,还具有以下几点有益效果:In the above-mentioned technical scheme, the equipment and process for rapidly realizing strip temperature transition in a continuous annealing furnace provided by the present invention also have the following beneficial effects:

1)本发明的设备及工艺技术通过在连续退火炉引入使用直火加热技术、电磁感应加热技术大幅度提高了带钢加热速度,和传统的连续退火炉相比,带钢加热速度从3-15℃/s提高到最高100-300℃/s;1) The equipment and process technology of the present invention greatly improves the heating speed of strip steel by introducing and using direct fire heating technology and electromagnetic induction heating technology in the continuous annealing furnace. Compared with the traditional continuous annealing furnace, the heating speed of strip steel is increased from 3- 15°C/s increased to a maximum of 100-300°C/s;

2)由于带钢加热速度得到大幅度提高,并且和传统的辐射管加热相比所使用的直火加热和电磁感应加热方式热惯性大幅度降低、当带钢的规格或退火温度发生变化时,可以通过快速调整直火加热的燃烧负荷和电磁感应加热的加热功率达到快速调整带钢温度的目的;2) Since the heating speed of the strip steel is greatly improved, and the thermal inertia of the direct fire heating and electromagnetic induction heating methods used is greatly reduced compared with the traditional radiant tube heating, when the specifications of the strip steel or the annealing temperature change, The purpose of quickly adjusting the strip temperature can be achieved by quickly adjusting the combustion load of direct fire heating and the heating power of electromagnetic induction heating;

3)基于以上两点的有益效果,在使用连续退火炉的实际生产中,带钢温度控制精度得到提高,温度不符的不良产品可以大幅度减少。3) Based on the beneficial effects of the above two points, in the actual production using the continuous annealing furnace, the temperature control accuracy of the strip steel is improved, and the defective products with inconsistent temperature can be greatly reduced.

附图说明Description of drawings

图1是现有连续退火炉的结构示意图;Fig. 1 is the structural representation of existing continuous annealing furnace;

图2是本发明设备实施例一的示意图;2 is a schematic diagram of Embodiment 1 of the device of the present invention;

图3是本发明设备实施例二的示意图;3 is a schematic diagram of Embodiment 2 of the device of the present invention;

图4是本发明设备实施例三的示意图;4 is a schematic diagram of Embodiment 3 of the device of the present invention;

图5是本发明设备实施例四的示意图。FIG. 5 is a schematic diagram of Embodiment 4 of the apparatus of the present invention.

具体实施方式Detailed ways

下面结合附图和实施例进一步说明本发明的技术方案。The technical solutions of the present invention are further described below with reference to the accompanying drawings and embodiments.

请结合图2至图5所示,本发明所提供的一种连续退火炉内快速实现带钢温度过渡的设备,包括:依次连接的加热段、横磁感应加热6、辐射管均热段7、缓冷段8和快冷段9,带钢10依次输送通过加热段、横磁感应加热6、辐射管均热段7、缓冷段8和快冷段9。Referring to Figures 2 to 5, a device for rapidly realizing strip temperature transition in a continuous annealing furnace provided by the present invention includes: a heating section connected in sequence, a transverse magnetic induction heating 6, a soaking section 7 of a radiant tube, Slow cooling section 8 and fast cooling section 9, strip steel 10 is transported through heating section, transverse magnetic induction heating 6, radiant tube soaking section 7, slow cooling section 8 and fast cooling section 9 in sequence.

较佳的,所述的加热段为依次连接的直火加热段11和辐射管加热段12。Preferably, the heating section is a direct-fire heating section 11 and a radiant tube heating section 12 that are connected in sequence.

较佳的,所述的加热段为直火加热段11。Preferably, the heating section is a direct-fire heating section 11 .

较佳的,所述的加热段为纵磁感应加热13。Preferably, the heating section is longitudinal magnetic induction heating 13 .

本发明还提供了一种连续退火炉内快速实现带钢温度过渡的工艺:The invention also provides a process for rapidly realizing the temperature transition of the strip in the continuous annealing furnace:

如图2所示,当带钢10温度小于600℃时,采用辐射管加热段12进行加热,由于带钢10温度相对较低,加热速度可达20-30℃/s;当带钢温10度大于600℃时,采用横磁感应加热6将带钢加热至目标温度,加热速度可达100-300℃/s;当带钢8的规格或退火曲线发生变化时,可以通过快速调整横磁感应加热6的加热功率达到快速调整带钢10温度的目的。As shown in Figure 2, when the temperature of the strip 10 is less than 600°C, the heating section 12 of the radiant tube is used for heating. Since the temperature of the strip 10 is relatively low, the heating rate can reach 20-30°C/s; When the temperature is higher than 600°C, the strip steel is heated to the target temperature by transverse magnetic induction heating 6, and the heating speed can reach 100-300°C/s; when the specification or annealing curve of strip steel 8 changes, the transverse magnetic induction heating can be quickly adjusted by adjusting the transverse magnetic induction heating. The heating power of 6 achieves the purpose of quickly adjusting the temperature of the strip steel 10.

如图3所示,当带钢10温度小于600℃时,采用直火加热段11进行加热,直火加热段10的加热速度可达50-100℃/s;当带钢10温度大于600℃时,采用辐射管加热段12继续将带钢10加热到700℃以下,加热速度可达20-30℃/s;当带钢10温度达到700℃以上时,采用横磁感应加热6将带钢10加热至目标温度,加热速度可达100-300℃/s;当带钢10的规格或退火曲线发生变化时,可以通过快速调整直火加热段11的燃烧负荷和横磁感应加热6的加热功率达到快速调整带钢10温度的目的。As shown in Fig. 3, when the temperature of the strip steel 10 is less than 600°C, the direct-fire heating section 11 is used for heating, and the heating speed of the direct-fire heating section 10 can reach 50-100°C/s; when the temperature of the strip steel 10 is greater than 600°C When the temperature of the steel strip 10 reaches 700°C or less, the heating speed of the steel strip 10 can reach 20-30°C/s; when the temperature of the steel strip 10 reaches above 700°C, the steel strip 10 is heated by the transverse magnetic induction heating 6. Heating to the target temperature, the heating speed can reach 100-300℃/s; when the specification of the strip steel 10 or the annealing curve changes, the combustion load of the direct fire heating section 11 and the heating power of the transverse magnetic induction heating 6 can be adjusted quickly to achieve The purpose of quickly adjusting the temperature of the strip 10.

如图4所示,当带钢10温度小于700℃时,采用直火加热段11进行加热,直火加热段10的加热速度可达50-100℃/s;当带钢10温度达到700℃以上时,采用横磁感应加热6将带钢10加热至目标温度,加热速度可达100-300℃/s;当带钢10的规格或退火曲线发生变化时,可以通过快速调整直火加热段11的燃烧负荷和横磁感应加热6的加热功率达到快速调整带钢10温度的目的。As shown in Fig. 4, when the temperature of the strip steel 10 is less than 700°C, the direct-fire heating section 11 is used for heating, and the heating rate of the direct-fire heating section 10 can reach 50-100°C/s; when the temperature of the strip steel 10 reaches 700°C In the above, the strip steel 10 is heated to the target temperature by the transverse magnetic induction heating 6, and the heating speed can reach 100-300°C/s; when the specification or annealing curve of the strip steel 10 changes, the direct fire heating section 11 can be quickly adjusted by adjusting The combustion load and the heating power of the transverse magnetic induction heating 6 achieve the purpose of quickly adjusting the temperature of the strip steel 10 .

如图5所示,利用纵磁感应加热13将带钢10加热至700℃,加热速度可达100-300℃/s;当带钢10温度达到700℃以上时,采用横磁感应加热6将带钢10加热至目标温度,加热速度可达100-300℃/s;当带钢10的规格或退火曲线发生变化时,可以通过快速调整纵磁感应加热13的加热功率和横磁感应加热6的加热功率达到快速调整带钢10温度的目的。As shown in Figure 5, the strip steel 10 is heated to 700°C by longitudinal magnetic induction heating 13, and the heating speed can reach 100-300°C/s; when the temperature of the strip steel 10 reaches above 700°C, the strip steel 10 is heated to the target temperature, and the heating speed can reach 100-300 ℃/s; when the specification or annealing curve of the strip steel 10 changes, the heating power of the longitudinal magnetic induction heating 13 and the heating power of the transverse magnetic induction heating 6 can be adjusted quickly to achieve The purpose of quickly adjusting the temperature of the strip 10.

综上所述,本发明的一种连续退火炉内快速实现带钢温度过渡的设备及工艺,使得带钢加热效率高、加热速度快,可以在生产中快速完成带钢温度切换,提高带钢温度控制精度,大幅度减少热处理温度不符造成的带钢性能不符发生量。To sum up, the equipment and process for rapidly realizing the temperature transition of the strip in the continuous annealing furnace of the present invention make the heating efficiency of the strip high and the heating speed fast, the temperature switching of the strip can be quickly completed in production, and the improvement of the strip temperature can be achieved. The precision of temperature control greatly reduces the occurrence of inconsistency in strip performance caused by inconsistency of heat treatment temperature.

通过本发明的设备及工艺对更加有效地控制带钢的热处理退火温度起到了非常积极有效的作用,在连续退火工艺的生产工艺和产品质量控制领域具有非常好的推广应用前景。The equipment and process of the invention play a very positive and effective role in controlling the heat treatment annealing temperature of the strip steel more effectively, and have a very good promotion and application prospect in the field of continuous annealing process production process and product quality control.

本技术领域中的普通技术人员应当认识到,以上的实施例仅是用来说明本发明,而并非用作为对本发明的限定,只要在本发明的实质精神范围内,对以上所述实施例的变化、变型都将落在本发明的权利要求书范围内。Those skilled in the art should realize that the above embodiments are only used to illustrate the present invention, but not to limit the present invention. Changes and modifications will fall within the scope of the claims of the present invention.

Claims (6)

1. The utility model provides an equipment of quick realization belted steel temperature transition in continuous annealing stove which characterized in that includes: the strip steel is sequentially conveyed to pass through the heating section, the transverse magnetic induction heating section, the radiant tube soaking section, the slow cooling section and the fast cooling section.
2. The apparatus for rapidly realizing the transition of the strip steel temperature in the continuous annealing furnace according to claim 1, characterized in that: the heating section is a direct fire heating section and a radiant tube heating section which are connected in sequence.
3. The apparatus for rapidly realizing the transition of the strip steel temperature in the continuous annealing furnace according to claim 1, characterized in that: the heating section is a direct-fire heating section.
4. The apparatus for rapidly realizing the transition of the strip steel temperature in the continuous annealing furnace according to claim 1, characterized in that: the heating section is used for longitudinal magnetic induction heating.
5. A process for rapidly achieving a strip temperature transition in a continuous annealing furnace according to any of claims 1 to 4, characterized in that:
when the temperature of the strip steel is less than 600 ℃, heating the strip steel by adopting a radiant tube heating section, when the temperature of the strip steel is more than 600 ℃, heating the strip steel to a target temperature by adopting transverse magnetic induction heating, and when the specification or the annealing curve of the strip steel is changed, adjusting the temperature of the strip steel by the heating power of the transverse magnetic induction heating;
when the temperature of the strip steel is less than 600 ℃, heating the strip steel by adopting a direct fire heating section, when the temperature of the strip steel is more than 600 ℃, continuously heating the strip steel to below 700 ℃ by adopting a radiant tube heating section, when the temperature of the strip steel reaches above 700 ℃, heating the strip steel to a target temperature by adopting transverse magnetic induction heating, and when the specification or annealing curve of the strip steel is changed, adjusting the temperature of the strip steel by using the combustion load of the direct fire heating section and the heating power of the transverse magnetic induction heating;
when the temperature of the strip steel is less than 700 ℃, heating the strip steel by adopting a direct fire heating section, when the temperature of the strip steel reaches above 700 ℃, heating the strip steel to a target temperature by adopting transverse magnetic induction heating, and when the specification or the annealing curve of the strip steel changes, adjusting the temperature of the strip steel by using the combustion load of the direct fire heating section and the heating power of the transverse magnetic induction heating;
the strip steel is heated to 700 ℃ by utilizing longitudinal magnetic induction heating, when the temperature of the strip steel reaches above 700 ℃, the strip steel is heated to a target temperature by adopting transverse magnetic induction heating, and when the specification or the annealing curve of the strip steel changes, the temperature of the strip steel is adjusted by the heating power of the longitudinal magnetic induction heating and the heating power of the transverse magnetic induction heating.
6. The process for rapidly realizing the temperature transition of the strip steel in the continuous annealing furnace according to claim 5, characterized in that: the heating speed of the heating section of the radiant tube is 20-30 ℃/s, the heating speed of transverse magnetic induction heating is 300 ℃/s, the heating speed of the direct-fire heating section is 50-100 ℃/s, and the heating speed of longitudinal magnetic induction heating is 300 ℃/s.
CN201910022891.3A 2019-01-10 2019-01-10 Equipment and process for quickly realizing temperature transition of strip steel in continuous annealing furnace Pending CN111424163A (en)