CN111254526A CN202010056952.0A CN202010056952A CN111254526A CN 111254526 A CN111254526 A CN 111254526A CN 202010056952 A CN202010056952 A CN 202010056952A CN 111254526 A CN111254526 A CN 111254526A
Authority
CN
China
Prior art keywords
wool
needle
speed
needles
combing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN202010056952.0A
Other languages
Chinese (zh)
Inventor
闻宇
胡建德
王术华
任亚平
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tianyu Wool Industry Zhangjiagang Free Trade Zone Co ltd
Original Assignee
Tianyu Wool Industry Zhangjiagang Free Trade Zone Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tianyu Wool Industry Zhangjiagang Free Trade Zone Co ltd filed Critical Tianyu Wool Industry Zhangjiagang Free Trade Zone Co ltd
Priority to CN202010056952.0A priority Critical patent/CN111254526A/en
Publication of CN111254526A publication Critical patent/CN111254526A/en
Pending legal-status Critical Current

Links

Classifications

    • DTEXTILES; PAPER
    • D01NATURAL OR MAN-MADE THREADS OR FIBRES; SPINNING
    • D01GPRELIMINARY TREATMENT OF FIBRES, e.g. FOR SPINNING
    • D01G13/00Mixing, e.g. blending, fibres; Mixing non-fibrous materials with fibres
    • DTEXTILES; PAPER
    • D02YARNS; MECHANICAL FINISHING OF YARNS OR ROPES; WARPING OR BEAMING
    • D02GCRIMPING OR CURLING FIBRES, FILAMENTS, THREADS, OR YARNS; YARNS OR THREADS
    • D02G3/00Yarns or threads, e.g. fancy yarns; Processes or apparatus for the production thereof, not otherwise provided for
    • D02G3/02Yarns or threads characterised by the material or by the materials from which they are made
    • D02G3/04Blended or other yarns or threads containing components made from different materials
    • D02G3/042Blended or other yarns or threads containing components made from different materials all components being made from natural material
    • DTEXTILES; PAPER
    • D10INDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES
    • D10BINDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES
    • D10B2211/00Protein-based fibres, e.g. animal fibres
    • D10B2211/01Natural animal fibres, e.g. keratin fibres
    • D10B2211/02Wool

Landscapes

  • Engineering & Computer Science (AREA)
  • Textile Engineering (AREA)
  • Mechanical Engineering (AREA)
  • Preliminary Treatment Of Fibers (AREA)

Abstract

The invention provides a wool top production method for improving the hand feeling of fabric, which comprises the following steps: 1) mixing hairs; 2) combing; 3) a front needle comb, 4) combing; 5) four needles; 6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 24-27, the vehicle speed is 30HZ, the pressure is 25-30, the feeding number is 8-10, the strip discharging weight is 25-27, and the strip discharging length is 50-55mm, and then repeating the step 5); 7) final needle; 8) and 7) mixing and spinning the product obtained in the step 7) with short wool. According to the production method of the wool tops for improving the fabric hand feeling, provided by the invention, the long wool is subjected to stretch-breaking treatment and then is blended with the short wool, so that the production cost is reduced, and the finally obtained wool tops are better in the fabric hand feeling during later processing.

Description

Wool top production method for improving fabric hand feeling
Technical Field
The invention relates to the field of textiles, in particular to a production method of wool tops for improving the hand feeling of fabrics.
Background
The wool is divided into long wool and short wool, because the price of the raw material of the short wool rises, the length of the long wool is longer, the original long wool and machine-made yarn are blended and used for manufacturing the fabric of the business suit, and the short wool has high wool content and plump hand feeling.
Disclosure of Invention
The invention aims to solve the problems in the prior art and provides a wool top production method for improving the hand feeling of a fabric.
In order to solve the technical problems, the technical scheme provided by the invention is as follows:
a wool top production method for improving fabric hand feeling comprises the following steps:
1) blending: the wool tops are chosen to be subjected to wool mixing, the type of the oil for the wool mixing is TCA, the type of the antistatic agent is 770, the antistatic agent amount is 2kg/t, and the wool amount is 1.5 t/h;
2) combing: the gross weight is 15-19g/m, the doffer speed is 44m/min, the cylinder speed is 490-510m/min, the working roller speed is 18m/min, the sliver discharging speed is 78-82m/min, the feeding roller speed is 0.2-0.3m/min, and the drafting multiple is 1.5;
3) front needle combing: the number of the first needles is 5, the second needles is 6, the third needles is 8, the gauge of the first needles is 32mm, the gauge of the second needles is 34mm and the gauge of the third needles is 38mm, the speed of the first needle is 200m/min, the speed of the second needle is 222m/min, the speed of the third needle is 230m/min, and the needle number: the head needle is round 3#, the second needle is round 4#, and the third needle is round 4 #;
4) combing: the number of the combined root of the two combing machines is 20 and 14 respectively, the number of the feeding teeth is 21, the combing speed is 180m/min, and the top comb needle number is 32 #;
5) four needles: the number of the combined roots is 7, the drafting multiple is 5.5-6.5, the speed is 220m/min, and the needle number is flat 5 #;
6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 24-27, the vehicle speed is 30HZ, the pressure is 25-30, the feeding number is 8-10, the strip discharging weight is 25-27, and the strip discharging length is 50-55mm, and then repeating the step 5);
7) final needling: the number of the combined roots is 7, the drafting multiple is 7-7.5, the speed is 220m/min, the needle number is flat No. 6, and the weight of the wool ball is 8.8-9.2 kg/kg;
8) and 7) mixing and spinning the product obtained in the step 7) with short wool.
As an improvement, the long wool tops in the step 1) are cleaned, and water is added before the wool oil and the antistatic agent are added, wherein the water addition standards are respectively 50kg/t and 8 kg/t.
As an improvement, water is added during the two-needle gilling, and the water adding amount is 25 ml/min.
The invention has the beneficial effects that:
the agricultural long wool is blended with the short wool after the stretch breaking treatment, so that the production cost is reduced, and the finally obtained wool top has better hand feeling during later processing.
Detailed Description
The invention is illustrated below by means of specific examples, without being restricted thereto.
Example one
A wool top production method for improving fabric hand feeling comprises the following steps:
1) blending: the wool tops are chosen to be subjected to wool mixing, the type of the oil for the wool mixing is TCA, the type of the antistatic agent is 770, the antistatic agent amount is 2kg/t, and the wool amount is 1.5 t/h;
2) combing: the gross weight is 15g/m, the doffer speed is 44m/min, the cylinder speed is 490m/min, the working roll speed is 18m/min, the sliver discharging speed is 78m/min, the feeding roll speed is 0.2m/min, and the drafting multiple is 1.5;
3) front needle combing: the number of the first needles is 5, the second needles is 6, the third needles is 8, the gauge of the first needles is 32mm, the gauge of the second needles is 34mm and the gauge of the third needles is 38mm, the speed of the first needle is 200m/min, the speed of the second needle is 222m/min, the speed of the third needle is 230m/min, and the needle number: the head needle is round 3#, the second needle is round 4#, and the third needle is round 4 #;
4) combing: the number of the combined root of the two combing machines is 20 and 14 respectively, the number of the feeding teeth is 21, the combing speed is 180m/min, and the top comb needle number is 32 #;
5) four needles: the number of the combined roots is 7, the drafting multiple is 5.5, the speed is 220m/min, and the needle number is flat 5 #;
6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 24, the vehicle speed is 30HZ, the pressure is 25, the feeding number is 8, the strip discharging weight is 25, the strip discharging length is 50mm, and then repeating the step 5);
7) final needling: the number of the combined roots is 7, the drafting multiple is 7-7.5, the speed is 220m/min, the needle number is flat No. 6, and the weight of the wool ball is 8.8 kg/kg;
8) and 7) mixing and spinning the product obtained in the step 7) with short wool.
Cleaning the long wool tops in the step 1), and adding water before adding the wool oil and the antistatic agent, wherein the water adding standards are respectively 50kg/t and 8 kg/t.
And adding water when the two-needle gilling is carried out, wherein the water adding amount is 25 ml/min.
Example two
A wool top production method for improving fabric hand feeling comprises the following steps:
1) blending: the wool tops are chosen to be subjected to wool mixing, the type of the oil for the wool mixing is TCA, the type of the antistatic agent is 770, the antistatic agent amount is 2kg/t, and the wool amount is 1.5 t/h;
2) combing: the gross weight is 19g/m, the doffer speed is 44m/min, the cylinder speed is 510m/min, the working roll speed is 18m/min, the sliver discharging speed is 82m/min, the feeding roll speed is 0.3m/min, and the drafting multiple is 1.5;
3) front needle combing: the number of the first needles is 5, the second needles is 6, the third needles is 8, the gauge of the first needles is 32mm, the gauge of the second needles is 34mm and the gauge of the third needles is 38mm, the speed of the first needle is 200m/min, the speed of the second needle is 222m/min, the speed of the third needle is 230m/min, and the needle number: the head needle is round 3#, the second needle is round 4#, and the third needle is round 4 #;
4) combing: the number of the combined root of the two combing machines is 20 and 14 respectively, the number of the feeding teeth is 21, the combing speed is 180m/min, and the top comb needle number is 32 #;
5) four needles: the number of the combined roots is 7, the drafting multiple is 5.5-6.5, the speed is 220m/min, and the needle number is flat 5 #;
6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 27, the vehicle speed is 30HZ, the pressure is 30, the number of the fed wool tops is 10, the strip discharging weight is 27, the strip discharging length is 55mm, and then repeating the step 5);
7) final needling: the number of the combined roots is 7, the drafting multiple is 7-7.5, the speed is 220m/min, the needle number is flat No. 6, and the weight of the wool ball is 9.2 kg/kg;
8) and 7) mixing and spinning the product obtained in the step 7) with short wool.
Cleaning the long wool tops in the step 1), and adding water before adding the wool oil and the antistatic agent, wherein the water adding standards are respectively 50kg/t and 8 kg/t.
And adding water when the two-needle gilling is carried out, wherein the water adding amount is 25 ml/min.
EXAMPLE III
A wool top production method for improving fabric hand feeling comprises the following steps:
1) blending: the wool tops are chosen to be subjected to wool mixing, the type of the oil for the wool mixing is TCA, the type of the antistatic agent is 770, the antistatic agent amount is 2kg/t, and the wool amount is 1.5 t/h;
2) combing: the weight of the wool is 17g/m, the doffer speed is 44m/min, the cylinder speed is 5000m/min, the working roll speed is 18m/min, the sliver discharging speed is 80m/min, the feeding roll speed is 0.25m/min, and the drafting multiple is 1.5;
3) front needle combing: the number of the first needles is 5, the second needles is 6, the third needles is 8, the gauge of the first needles is 32mm, the gauge of the second needles is 34mm and the gauge of the third needles is 38mm, the speed of the first needle is 200m/min, the speed of the second needle is 222m/min, the speed of the third needle is 230m/min, and the needle number: the head needle is round 3#, the second needle is round 4#, and the third needle is round 4 #;
4) combing: the number of the combined root of the two combing machines is 20 and 14 respectively, the number of the feeding teeth is 21, the combing speed is 180m/min, and the top comb needle number is 32 #;
5) four needles: the number of the combined roots is 7, the drafting multiple is 5.5-6.5, the speed is 220m/min, and the needle number is flat 5 #;
6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 25, the vehicle speed is 30HZ, the pressure is 27, the feeding quantity is 90, the top weight is 26, the top length is 52mm, and then repeating the step 5);
7) final needling: the number of the combined roots is 7, the drafting multiple is 7.2, the speed is 220m/min, the needle number is flat 6#, and the weight of the wool ball is 9 kg/kg;
8) and 7) mixing and spinning the product obtained in the step 7) with short wool.
Cleaning the long wool tops in the step 1), and adding water before adding the wool oil and the antistatic agent, wherein the water adding standards are respectively 50kg/t and 8 kg/t.
And adding water when the two-needle gilling is carried out, wherein the water adding amount is 25 ml/min.
The above description is only for the preferred embodiment of the present invention, but the scope of the present invention is not limited thereto, and any person skilled in the art should be considered to be within the technical scope of the present invention, and the technical solutions and the inventive concepts thereof according to the present invention should be equivalent or changed within the scope of the present invention.

Claims (3)

1. A wool top production method for improving fabric hand feeling is characterized by comprising the following steps:
1) blending: the wool tops are chosen to be subjected to wool mixing, the type of the oil for the wool mixing is TCA, the type of the antistatic agent is 770, the antistatic agent amount is 2kg/t, and the wool amount is 1.5 t/h;
2) combing: the gross weight is 15-19g/m, the doffer speed is 44m/min, the cylinder speed is 490-510m/min, the working roller speed is 18m/min, the sliver discharging speed is 78-82m/min, the feeding roller speed is 0.2-0.3m/min, and the drafting multiple is 1.5;
3) front needle combing: the number of the first needles is 5, the second needles is 6, the third needles is 8, the gauge of the first needles is 32mm, the gauge of the second needles is 34mm and the gauge of the third needles is 38mm, the speed of the first needle is 200m/min, the speed of the second needle is 222m/min, the speed of the third needle is 230m/min, and the needle number: the head needle is round 3#, the second needle is round 4#, and the third needle is round 4 #;
4) combing: the number of the combined root of the two combing machines is 20 and 14 respectively, the number of the feeding teeth is 21, the combing speed is 180m/min, and the top comb needle number is 32 #;
5) four needles: the number of the combined roots is 7, the drafting multiple is 5.5-6.5, the speed is 220m/min, and the needle number is flat 5 #;
6) breaking by pulling: feeding four needles of back wool tops, wherein the gram weight is 24-27, the vehicle speed is 30HZ, the pressure is 25-30, the feeding number is 8-10, the strip discharging weight is 25-27, and the strip discharging length is 50-55mm, and then repeating the step 5);
7) final needling: the number of the combined roots is 7, the drafting multiple is 7-7.5, the speed is 220m/min, the needle number is flat No. 6, and the weight of the wool ball is 8.8-9.2 kg/kg;
8) and 7) mixing and spinning the product obtained in the step 7) with short wool.
2. The method for producing wool tops with improved fabric hand feeling according to claim 1, wherein the long wool tops in the step 1) are cleaned, and are treated by adding water before adding wool oil and an antistatic agent, wherein the water addition standard is 50kg/t and 8kg/t respectively.
3. The method for producing wool tops by using the knitted fabric with improved handfeel as claimed in claim 1, wherein water is added during the two-needle carding, and the water addition amount is 25 ml/min.
CN202010056952.0A 2020-01-16 2020-01-16 Wool top production method for improving fabric hand feeling Pending CN111254526A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN202010056952.0A CN111254526A (en) 2020-01-16 2020-01-16 Wool top production method for improving fabric hand feeling

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN202010056952.0A CN111254526A (en) 2020-01-16 2020-01-16 Wool top production method for improving fabric hand feeling

Publications (1)

Publication Number Publication Date
CN111254526A true CN111254526A (en) 2020-06-09

Family

ID=70944108

Family Applications (1)

Application Number Title Priority Date Filing Date
CN202010056952.0A Pending CN111254526A (en) 2020-01-16 2020-01-16 Wool top production method for improving fabric hand feeling

Country Status (1)

Country Link
CN (1) CN111254526A (en)

Citations (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1480571A (en) * 2002-09-05 2004-03-10 上海第十七棉纺织总厂 Blended yarm among cotton, modat and wool as well as processing procedure
CN101469470A (en) * 2007-12-28 2009-07-01 天津纺织工程研究院有限公司 Wool semi-worsted spinning technique
US20100252138A1 (en) * 2009-04-06 2010-10-07 Tseng Kun-Yu Method of making a textile product from a fiber blend including wool fibers and a woven textile product made therefrom
CN103757777A (en) * 2014-01-22 2014-04-30 宁波康赛妮毛绒制品有限公司 Cashmere and stretched wool blended yarn and manufacturing method thereof
CN105088451A (en) * 2014-05-23 2015-11-25 天津纺织工程研究院有限公司 A stretched wool/cotton colored spun yarn technology
CN107217353A (en) * 2017-06-16 2017-09-29 江苏中孚达科技股份有限公司 A kind of spinning process of superelevation branch silk/yakwool/wool yarns
CN110144652A (en) * 2019-06-06 2019-08-20 张家港扬子纺纱有限公司 A kind of ultra-fine tencel wool blended yarn preparation method
CN110644097A (en) * 2019-10-22 2020-01-03 江苏阳光股份有限公司 Preparation method of superfine tencel and wool blended yarn

Patent Citations (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1480571A (en) * 2002-09-05 2004-03-10 上海第十七棉纺织总厂 Blended yarm among cotton, modat and wool as well as processing procedure
CN101469470A (en) * 2007-12-28 2009-07-01 天津纺织工程研究院有限公司 Wool semi-worsted spinning technique
US20100252138A1 (en) * 2009-04-06 2010-10-07 Tseng Kun-Yu Method of making a textile product from a fiber blend including wool fibers and a woven textile product made therefrom
CN103757777A (en) * 2014-01-22 2014-04-30 宁波康赛妮毛绒制品有限公司 Cashmere and stretched wool blended yarn and manufacturing method thereof
CN105088451A (en) * 2014-05-23 2015-11-25 天津纺织工程研究院有限公司 A stretched wool/cotton colored spun yarn technology
CN107217353A (en) * 2017-06-16 2017-09-29 江苏中孚达科技股份有限公司 A kind of spinning process of superelevation branch silk/yakwool/wool yarns
CN110144652A (en) * 2019-06-06 2019-08-20 张家港扬子纺纱有限公司 A kind of ultra-fine tencel wool blended yarn preparation method
CN110644097A (en) * 2019-10-22 2020-01-03 江苏阳光股份有限公司 Preparation method of superfine tencel and wool blended yarn

Non-Patent Citations (3)

* Cited by examiner, † Cited by third party
Title
Б•В•奥泽洛夫: "《精梳毛纺梳毛机》", 29 February 1960, 纺织工业出版社 *
范尧明: "《70支澳毛条的生产控制与TEAM2预测》", 《毛纺科技》 *
郁崇文: "《纺纱工艺学》", 31 August 2015, 东华大学出版社 *

Similar Documents

Publication Publication Date Title
CN102719961B (en) Antibacterial blended yarn and spinning process thereof
CN102517737B (en) Wool yarn and production process thereof
EP1598458B1 (en) Yarn comprising bamboo fibers and method for making the same
CN104480590B (en) A kind of Yarn spinning method of high-count spun silk yarn yarn
CN102021703A (en) Silver fiber and cotton blended knitting yarn and preparation method thereof
CN105755622A (en) Rough-yarn-method AB yarn production technology
CN110699807B (en) High-proportion worsted velvet product and preparation method thereof
CN102704098B (en) Production process of pure-spined combed yak wool
CN105821544A (en) Yarn spinning process of high-count combed pure mohair knitted yarns
CN110055651A (en) The scribbled and its spinning process of Sorona fiber, Seawool fiber and regenerated terylene
CN110129945A (en) A kind of production method of anti-bacterial blended yarn
CN103741305B (en) Scribbled containing Herba Pileae Scriptae fiber and mint fibers and preparation method thereof
CN104805560A (en) Hygroscopic, breathable and antibacterial ultra-high molecular weight polyethylene blended core spun yarn and production method thereof
CN101748529A (en) Scribbled of banana fiber and production method thereof
CN104711729A (en) Blended yarn of all-new ultra-mimic cotton fibers and mercerized wool fibers and spinning process thereof
CN114016173A (en) Spinning production process of domestic animal hair and down and domestic polylactic acid fiber blended yarn
CN108728961A (en) A kind of cashmere water soluble fiber mixing spinning method for genuine
CN113403719B (en) Elastic short fiber pure spun yarn of comfortable elastic silk and production process thereof
CN101586278A (en) Cashmere yarn with high tensile stretch and production technology thereof
CN110846762A (en) Production method of luoma-hair blended fiber product
CN100415969C (en) Cotton flax blended yarn with high yarn counts and its manufacturing process
CN113737334A (en) Domestic animal hair and down and domestic polylactic acid fiber blended yarn and ring spinning production process
CN111254526A (en) Wool top production method for improving fabric hand feeling
CN105420871A (en) 120 Nm/3 spun silk and cotton mixed plied yarn and production method thereof
CN104674400A (en) Method for spinning fine count yarns by use of pure cashmere fibers

Legal Events

Date Code Title Description
PB01 Publication
PB01 Publication
SE01 Entry into force of request for substantive examination
SE01 Entry into force of request for substantive examination
RJ01 Rejection of invention patent application after publication
RJ01 Rejection of invention patent application after publication

Application publication date: 20200609