CN108655370A - A kind of composite plate blanks casting method and device - Google Patents
A kind of composite plate blanks casting method and device Download PDFInfo
- Publication number
- CN108655370A CN108655370A CN201810473657.8A CN201810473657A CN108655370A CN 108655370 A CN108655370 A CN 108655370A CN 201810473657 A CN201810473657 A CN 201810473657A CN 108655370 A CN108655370 A CN 108655370A
- Authority
- CN
- China
- Prior art keywords
- casting
- trolley
- composite plate
- plate blanks
- guide rail
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
技术领域technical field
本发明涉及一种复合板坯铸造方法及装置。The invention relates to a composite slab casting method and device.
背景技术Background technique
常规合金由于性能单一,不能很好满足如运载工具、结构、电子等工程方面的多种性能综合的要求,因此复合材料成为新材料研发的重点。层状复合材料由于成本低、综合性能好,是应用广泛、生产量最大的复合材料,其中复合板带材则是目前用量最多的复合材料。Due to the single performance of conventional alloys, they cannot well meet the comprehensive requirements of multiple performances in engineering such as vehicles, structures, and electronics. Therefore, composite materials have become the focus of new material research and development. Due to its low cost and good overall performance, layered composite materials are the most widely used composite materials with the largest production volume, and the composite sheet and strip are currently the most used composite materials.
复合板带材的主要生产方法可以分成三类:一类为固相复合法,包括热轧复合,冷轧复合等,第二类为液固复合法,如反向凝固法等,第三类为液态复合法,如连续浇铸法。传统的复合板带材的生产技术是轧制复合,在高温大压率下创造更多的新表面来实现复合,但它们的缺点是:浇铸是将钢液从钢水包浇入中间包,而钢液的获得需要铁水及废钢中含有C、Mn、Si、P、S等杂质,在低温融化过程中,C、Si、P、S被氧化,使单质态的杂质变为化合态的杂质,以利于后期进一步去除杂质。氧来源于炉料中的铁锈(成分为Fe2O3·2H2O)、氧化铁皮、加入的铁矿石以及空气中的氧和吹氧。各种杂质的氧化过程是在炉渣与钢液的界面之间进行的。氧化过程是在高温下进行的脱炭、去磷、去气、去杂质反应、脱氧、脱硫与出钢。氧化末期,钢中含有大量过剩的氧,通过向钢液中加入块状或粉状铁合金或多元素合金来去除钢液中过剩的氧,产生的有害气体CO随炉气排出,产生的炉渣可进一步脱硫,即在最后的出钢过程中,渣、钢强烈混合冲洗,增加脱硫反应。从炼钢炉中冶炼出来的钢水含有少量的气体及杂质,一般是将钢水注入精炼包中,进行吹氩、脱气、钢包精炼等工序,得到较纯净的钢液。The main production methods of composite plates and strips can be divided into three categories: one is solid-phase composite method, including hot rolling composite, cold rolling composite, etc., the second is liquid-solid composite method, such as reverse solidification method, etc., and the third category is It is a liquid composite method, such as continuous casting. The traditional production technology of clad plate and strip is rolling and cladding, which creates more new surfaces under high temperature and high pressure rate to achieve cladding, but their disadvantages are: casting is to pour molten steel from ladle into tundish, and The acquisition of molten steel requires impurities such as C, Mn, Si, P, and S in the molten iron and scrap steel. During the low-temperature melting process, C, Si, P, and S are oxidized, so that the impurities in the single state become the impurities in the combined state. In order to facilitate the further removal of impurities in the later stage. Oxygen comes from rust in the furnace charge (the composition is Fe 2 O 3 ·2H 2 O), iron oxide scale, added iron ore, oxygen in the air and blown oxygen. The oxidation process of various impurities is carried out between the interface of slag and molten steel. The oxidation process is decarburization, dephosphorization, degassing, impurity removal reaction, deoxidation, desulfurization and tapping carried out at high temperature. At the end of oxidation, the steel contains a large amount of excess oxygen, and the excess oxygen in the molten steel is removed by adding block or powdered ferroalloy or multi-element alloy to the molten steel, and the harmful gas CO produced is discharged with the furnace gas, and the slag produced can be Further desulfurization, that is, in the final tapping process, the slag and steel are strongly mixed and washed to increase the desulfurization reaction. The molten steel smelted from the steelmaking furnace contains a small amount of gas and impurities. Generally, the molten steel is poured into the refining ladle, and argon blowing, degassing, ladle refining and other processes are performed to obtain relatively pure molten steel.
在材料加工领域,尤其是复合浇铸过程中,避免钢液被氧化是复合浇铸工艺的最基本最重要的目标。然而在实际过程中,钢液在浇铸过程中不可避免的接触空气、耐材、覆盖剂等物质,其中接触空气产生的氧化对最终复合钢材的质量影响最大,同时也是最难控制的,导致在钢液浇铸在模具里的同时,就已经发生氧化,严重时导致钢液结瘤无法继续进行浇注。In the field of material processing, especially in the composite casting process, avoiding the oxidation of molten steel is the most basic and important goal of the composite casting process. However, in the actual process, molten steel inevitably contacts air, refractory materials, covering agents and other substances during the casting process, among which the oxidation caused by contact with air has the greatest impact on the quality of the final composite steel, and is also the most difficult to control, resulting in While the molten steel is being cast in the mold, oxidation has already occurred, and in severe cases, the molten steel nodules cannot continue to be poured.
申请号为201110100831.2的中国专利公开了了一种铝合金复合铸锭的连铸方法及其装置,属于铝合金铸造技术领域,将待复合的两种合金分别熔炼,向冷却板水腔和水箱内通入冷却水并保持水流动,将芯材合金液导入芯材熔体腔,启动引锭开始铸造,能够保证表材合金液体流动均匀,液面稳定,温度均匀,确保复合面的全面冶金结合;申请号为201510462834.9的中国专利公开了一种铜铝复合铸造用的二次冷却装置,可以满足铝芯铸造的冷却条件,冷却强度和精度都较高,极大提升铸坯铜铝结合性能;申请号为201210513238.5的中国专利公开了一种铝铜复合板及其制备方法,通过控制厚度,铝层代替了部分铜层,降低了材料成本,具有较小的比重。The Chinese patent application number 201110100831.2 discloses a continuous casting method and device for aluminum alloy composite ingots, which belongs to the field of aluminum alloy casting technology. Put in cooling water and keep the water flowing, introduce the core material alloy liquid into the core material melt cavity, start the dummy ingot to start casting, which can ensure the surface material alloy liquid flows evenly, the liquid level is stable, and the temperature is uniform, ensuring the comprehensive metallurgical bonding of the composite surface ; The Chinese patent application number 201510462834.9 discloses a secondary cooling device for copper-aluminum composite casting, which can meet the cooling conditions of aluminum core casting, has high cooling intensity and precision, and greatly improves the bonding performance of copper-aluminum casting billets; The Chinese patent application number 201210513238.5 discloses an aluminum-copper composite board and its preparation method. By controlling the thickness, the aluminum layer replaces part of the copper layer, which reduces the material cost and has a smaller specific gravity.
以上阐述的方法可以生产出质量较好的复合铸锭,但是由于液面控制环节太多,操作复杂,配合较困难,表材液面容易形成虚焊,最关键处在于无法根除由于氧化迅速导致钢液结瘤无法继续进行浇注的问题。The method described above can produce composite ingots with better quality, but because there are too many liquid level control links, the operation is complicated, and the coordination is difficult, the liquid surface of the surface material is easy to form virtual welding. The most critical point is that it cannot be eradicated due to rapid oxidation. The problem that molten steel nodules cannot continue pouring.
发明内容Contents of the invention
为克服现有技术的不足,本发明的目的是提供一种复合板坯铸造方法及装置,用于制造两种钢种的复合板材,减少杂质的产生,提高复合板坯的质量。In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a composite slab casting method and device for manufacturing composite slabs of two steel types, reducing the generation of impurities and improving the quality of the composite slab.
为实现上述目的,本发明通过以下技术方案实现:To achieve the above object, the present invention is achieved through the following technical solutions:
一种复合板坯铸造装置,包括箱体、导轨、浇注小车,箱体顶部固定有导轨,浇注小车走行在导轨上,浇注小车由电动机驱动;所述的箱体内壁上铺设有耐火砖。A composite slab casting device, comprising a box body, a guide rail, and a pouring trolley, the top of the box body is fixed with a guide rail, the pouring trolley runs on the guide rail, and the pouring trolley is driven by a motor; the inner wall of the box is laid with refractory bricks.
所述的导轨由两根相互平行的金属导轨组成。The guide rail is composed of two metal guide rails parallel to each other.
所述箱体侧壁设有若干喷孔。The side wall of the box body is provided with several spray holes.
一种复合板坯铸造方法,包括以下步骤:A composite slab casting method, comprising the following steps:
1)将待复合的两种合金分别熔炼,然后精炼,将获得的两种合金液分别静置;1) Melting the two alloys to be compounded respectively, then refining, and standing the two obtained alloy liquids separately;
2)一种合金液通过钢包铸入浇注小车,由浇注小车将合金液铸入箱体,通过浇注小车将呈熔融态的合金铺满整个金属箱体的底部;然后将保护剂和保护砂填入浇注小车,利用小车移动把保护砂注入箱体中,两次过程保证浇注小车速度一致,使合金液落下后来不及发生氧化就会被保护剂覆盖;最后浇注小车将另一种合金液浇铸到保护剂上;在整个浇铸过程中,向箱体内持续通氮气或氩气;2) An alloy liquid is cast into the pouring trolley through the ladle, the alloy liquid is cast into the box by the pouring trolley, and the molten alloy is covered with the bottom of the entire metal box by the pouring trolley; then the protective agent and protective sand are filled Enter the pouring trolley, and use the trolley to move the protective sand into the box. The two processes ensure that the speed of the pouring trolley is consistent, so that the alloy liquid will be covered by the protective agent before oxidation occurs after it falls; finally, the pouring trolley casts another alloy liquid into the On the protective agent; throughout the casting process, nitrogen or argon is continuously passed into the box;
3)在保护气体环境下,用高压气除去保护剂、保护砂及氧化杂质,最后经冷却结晶得到复合板材。3) Under the protective gas environment, use high-pressure gas to remove the protective agent, protective sand and oxidized impurities, and finally obtain the composite plate through cooling and crystallization.
步骤2)中浇注小车的浇注速度保持在50~70mm/s。The pouring speed of the pouring trolley in step 2) is kept at 50-70mm/s.
步骤2)浇注小车的浇注合金液的速度为120~180kg/min。Step 2) The speed of pouring the molten alloy in the pouring trolley is 120-180kg/min.
所述的保护剂由萤石和石化组成,其中萤石按质量百分比占保护剂的5%~8%;保护剂的粒径为4-6mm。The protective agent is composed of fluorite and petrochemicals, wherein the fluorite accounts for 5%-8% of the protective agent by mass percentage; the particle size of the protective agent is 4-6mm.
所述的保护砂为硼砂,硼砂的粒径为1-3mm。The protective sand is borax, and the particle diameter of borax is 1-3mm.
所述的保护气为氮气或氩气。The protective gas is nitrogen or argon.
与现有技术相比,本发明的有益效果是:Compared with prior art, the beneficial effect of the present invention is:
本发明通过喷涂保护气和保护砂两种方法,可以给予钢液一种致密的保护气氛,而且保护砂由于覆盖在钢液表面,这种覆盖率可以高达97%以上,可以有效排除环境中的氧化性气体对高温金属的氧化影响,氧化率降到10%以内,从而有效避免氧化铁皮的产生。此外,由于复合板坯铸造装置中,浇注小车经电机驱动实现了可移动性,熔融金属在浇铸过程中很大程度上处于流动状态,有效解决了浇铸过程中“死区”的产生,保证浇铸成品的内部组织更加致密均匀,提高了复合板材的质量。The present invention can give the molten steel a dense protective atmosphere by spraying protective gas and protective sand, and since the protective sand covers the surface of the molten steel, the coverage rate can be as high as 97%, which can effectively eliminate environmental pollution. Oxidizing gas has an effect on the oxidation of high-temperature metals, and the oxidation rate is reduced to less than 10%, thus effectively avoiding the generation of oxidized iron scale. In addition, because in the composite slab casting device, the pouring trolley is driven by a motor to achieve mobility, and the molten metal is largely in a flowing state during the casting process, which effectively solves the "dead zone" in the casting process and ensures that the casting The internal organization of the finished product is denser and more uniform, which improves the quality of the composite board.
附图说明Description of drawings
图1是复合板坯铸造装置的结构示意图。Fig. 1 is a structural schematic diagram of a composite slab casting device.
图2是浇注小车的结构示意图。Figure 2 is a schematic structural view of the pouring trolley.
图中:1-电动机驱动装置 2-浇注小车 3-箱体 4-不锈钢 5-导轨 6-保护剂和保护砂 7-碳钢 201-支架 202-挡板焊接件 203-钢包 204-金属钢架 205-耐火材料层 206-承液管 207-中间包 208-漏液口 209-铁水包耳 210-电子秤 211-电线。In the figure: 1-motor drive device 2-pouring trolley 3-box body 4-stainless steel 5-guide rail 6-protective agent and protective sand 7-carbon steel 201-bracket 202-baffle plate weldment 203-steel ladle 204-metal steel frame 205-refractory material layer 206-liquid receiving pipe 207-tundish 208-leakage port 209-hot metal bag ear 210-electronic scale 211-wire.
具体实施方式Detailed ways
下面结合说明书附图对本发明进行详细地描述,但是应该指出本发明的实施不限于以下的实施方式。The present invention will be described in detail below in conjunction with the accompanying drawings, but it should be pointed out that the implementation of the present invention is not limited to the following embodiments.
见图1,复合板坯铸造装置,包括箱体3、导轨5、浇注小车2,箱体3顶部固定有导轨5,浇注小车2走行在导轨5上,浇注小车2由电动机1驱动;箱体3内壁上铺设有耐火砖。导轨5由两根相互平行的金属导轨5组成,两根金属导轨5之间的距离与浇注小车2的车轮距离相对应。箱体3用于承接从漏液口208流出的钢液。箱体3侧壁设有若干喷孔,用以喷吹保护气。As shown in Figure 1, the composite slab casting device includes a box body 3, a guide rail 5, and a pouring trolley 2. The top of the box body 3 is fixed with a guide rail 5, and the pouring trolley 2 runs on the guide rail 5. The pouring trolley 2 is driven by a motor 1; 3 Refractory bricks are laid on the inner wall. The guide rail 5 is made up of two metal guide rails 5 parallel to each other, and the distance between the two metal guide rails 5 corresponds to the wheel distance of the pouring trolley 2 . The box body 3 is used to receive the molten steel flowing out from the liquid leakage port 208 . The side wall of the box body 3 is provided with a number of nozzle holes for blowing protective gas.
见图2,浇注小车2包括支架201、电动机驱动装置1、挡板焊接件202、电线211、钢包203、金属钢架204、承液管206、中间包207、漏液口208、铁水包耳209、电子秤210,支架201固定在下部支撑平台上,支架201位于箱体3正上方,支架201与箱体3顶部的距离为300-350mm;支架201与金属钢架204固定连接,支架201通过电动机驱动装置1驱动在导轨5上移动;电动机驱动装置1主要由滚轮、电动机组成,电动机固定在支架201上,滚轮设置在支架201上,滚轮由电动机驱动,滚轮在导轨5上滚动,实现驱动浇注小车2移动的目的;钢包203和中间包207设置在金属钢架204上,钢包203承接浇注液,钢包203两侧固定有铁水包耳209,钢包203通过铁水包耳209放置在金属钢架204上,钢包203下面设置有中间包207,耐火材料层205置于钢包203和中间包207之间,并固定在中间包207上,耐火材料层205厚度为8mm以上;As shown in Figure 2, the pouring trolley 2 includes a bracket 201, a motor drive device 1, a baffle weldment 202, an electric wire 211, a ladle 203, a metal steel frame 204, a liquid receiving pipe 206, a tundish 207, a liquid leakage port 208, and molten iron ladle ears 209. Electronic scale 210, the bracket 201 is fixed on the lower support platform, the bracket 201 is located directly above the box body 3, the distance between the bracket 201 and the top of the box body 3 is 300-350mm; the bracket 201 is fixedly connected with the metal steel frame 204, and the bracket 201 Driven by the motor drive device 1 to move on the guide rail 5; the motor drive device 1 is mainly composed of a roller and a motor. The purpose of driving the pouring trolley 2 to move; the ladle 203 and the tundish 207 are set on the metal steel frame 204, the ladle 203 accepts the pouring liquid, the two sides of the ladle 203 are fixed with ladle ears 209, and the ladle 203 is placed on the metal steel frame through the ladle ears 209 On the frame 204, a tundish 207 is arranged under the steel ladle 203, the refractory material layer 205 is placed between the steel ladle 203 and the tundish 207, and fixed on the tundish 207, and the thickness of the refractory material layer 205 is more than 8mm;
钢包203内设有承液管206,承液管206底部延伸到中间包207内,中间包207底部设有漏液口208,漏液口208上连接有阀门;电子秤210设置在金属钢架204边缘上;支架201与金属钢架204之间焊接有挡板焊接件202,用于固定支架201与金属钢架204;电线211连接电源用于电子秤210和电动机驱动装置1供电;The ladle 203 is provided with a liquid receiving pipe 206, and the bottom of the liquid receiving pipe 206 extends into the tundish 207, and the bottom of the tundish 207 is provided with a liquid leakage port 208, and a valve is connected to the liquid leakage port 208; the electronic scale 210 is set on a metal steel frame On the edge of 204; a baffle weldment 202 is welded between the bracket 201 and the metal steel frame 204 for fixing the bracket 201 and the metal steel frame 204; the electric wire 211 is connected to the power supply for the electronic scale 210 and the motor drive device 1;
其中,金属钢架204的尺寸为1500×10000×500mm,用来放置钢包203和中间包207。Wherein, the size of the metal steel frame 204 is 1500×10000×500 mm, which is used to place the steel ladle 203 and the tundish 207 .
复合板坯铸造方法,包括以下步骤:Composite slab casting method, comprising the following steps:
1)将待复合的两种合金分别熔炼,然后精炼,将获得的两种合金液分别在钢包203中静置。1) The two alloys to be compounded are melted separately, and then refined, and the obtained two alloy liquids are placed in the ladle 203 to stand still.
2)一种合金液通过钢包203铸入浇注小车2,由浇注小车2将合金液铸入箱体3,通过移动式的浇注小车2将呈熔融态的合金铺满整个金属箱体3的底部;之后,将所用到的保护剂和保护砂6填满浇注小车2,再次利用小车将保护剂和保护砂6铺在合金的表面,两次浇铸过程保证浇注小车2速度一致,使合金液落下后来不及发生氧化就会被保护砂覆盖;最后浇注小车2将另一种合金液浇铸到保护剂上;在整个浇铸过程中,向箱体3内持续通保护气;浇注小车2的浇铸速度保持在50~70mm/s。浇注小车2的浇铸合金液的速度为120~180kg/min。2) An alloy liquid is cast into the pouring trolley 2 through the ladle 203, the alloy liquid is cast into the box body 3 by the pouring trolley 2, and the molten alloy is spread over the bottom of the entire metal box body 3 by the mobile pouring trolley 2 ; After that, fill the pouring trolley 2 with the protective agent and protective sand 6 used, and spread the protective agent and protective sand 6 on the surface of the alloy with the trolley again. The two casting processes ensure that the pouring trolley 2 has the same speed, so that the alloy liquid falls Later, it will be covered with protective sand before oxidation occurs; finally, the pouring trolley 2 casts another alloy liquid onto the protective agent; during the entire casting process, the protective gas is continuously passed into the box 3; the casting speed of the pouring trolley 2 maintains At 50-70mm/s. The speed of pouring the molten alloy in the trolley 2 is 120-180kg/min.
3)在保护气体环境下,用高压气除去保护剂、保护砂及氧化杂质,最后经冷却结晶得到复合板材。所用到的高压气,气压一般不超过20MPa,吹扫整个箱体3,持续时间固定在60s以内。其中,保护剂由萤石和石化组成,其中萤石按质量百分比占保护剂的5%~8%。保护剂的粒径维持在5±1mm,保护剂使钢液中浮渣效果增强,萤石的主要作用是稀释炉渣,降低炉渣的熔点,提高炉渣的流动性。保护砂为硼砂,硼砂的粒径尽量保持在2±1mm,可以清除金属表面的氧化物。保护气为氮气或氩气,保护气主要是氮气,而且氮气纯度要求99.99%以上;此外,还可以在浇铸过程中吹入氩气,使成分均匀,钢液净化,并可除掉溶解在钢中的氢、氮、氧等杂质,提高质量,吹入氩气还可以缩短冶炼时间,提高产量,节约电能。其中,保护剂与保护砂的加入量可按照1∶(0.8-1.2)的重量比。3) Under the protective gas environment, use high-pressure gas to remove the protective agent, protective sand and oxidized impurities, and finally obtain the composite plate through cooling and crystallization. The high-pressure gas used generally does not exceed 20MPa, and the entire box body 3 is purged, and the duration is fixed within 60s. Wherein, the protective agent is composed of fluorite and petrochemical, wherein the fluorite accounts for 5% to 8% of the protective agent by mass percentage. The particle size of the protective agent is maintained at 5±1mm. The protective agent enhances the scum effect in the molten steel. The main function of fluorite is to dilute the slag, reduce the melting point of the slag, and improve the fluidity of the slag. The protective sand is borax, and the particle size of borax should be kept at 2±1mm as much as possible, which can remove oxides on the metal surface. The protective gas is nitrogen or argon, the protective gas is mainly nitrogen, and the purity of nitrogen must be more than 99.99%; in addition, argon can also be blown in during the casting process to make the composition uniform, purify the molten steel, and remove the dissolved steel. Impurities such as hydrogen, nitrogen, and oxygen in the furnace can improve the quality, and blowing in argon can also shorten the smelting time, increase the output, and save electric energy. Wherein, the addition amount of protective agent and protective sand can be according to the weight ratio of 1: (0.8-1.2).
实施例1Example 1
见图1,箱体3尺寸为2000×8000×2000mm,箱体3选择高强度耐高温的合金板材,导轨5横搭在箱体3上,两根金属导轨5的间距与浇注小车2的车轮间距相适应,即为1000mm;浇注小车2可选用2000×2000×1000mm的尺寸;复合板坯铸造方法,包括以下步骤:As shown in Figure 1, the size of the box body 3 is 2000×8000×2000mm. The box body 3 is made of high-strength and high-temperature-resistant alloy plates. The guide rail 5 is placed horizontally on the box body 3. The spacing is adapted, that is, 1000mm; the size of the pouring trolley 2 can be 2000×2000×1000mm; the composite slab casting method includes the following steps:
1)将待复合的两种合金,不锈钢4和碳钢7,分别熔炼,然后精炼,将获得的两种合金液分别在钢包203中静置。1) The two alloys to be compounded, stainless steel 4 and carbon steel 7, are melted separately, and then refined, and the obtained two alloy liquids are placed in the ladle 203 respectively.
2)将不锈钢4金属液通过钢包203铸入浇注小车2,浇注小车2开始以60mm/s进行往复移动,先由浇注小车2将不锈钢4金属液铸入箱体3,通过浇注小车2将呈熔融态的不锈钢4铺满整个金属箱体3的底部;然后将硼砂6装入浇注小车2利用小车的移动性铺在不锈钢4的表面,两次浇铸过程保证浇注小车2速度一致,使不锈钢4液落下后来不及发生氧化就会被保护剂覆盖;最后浇注小车2将制得的1600℃高温的碳钢7金属液800kg,浇铸到保护剂上;在整个浇铸过程中,向箱体3内持续通保护气,两种钢液落下后来不及被氧气氧化就会被保护气和保护砂覆盖笼罩,有效防止钢液由于高温而被瞬间氧化;浇注小车2的浇铸速度保持在50~70mm/s。钢液会在小车单方向移动一次就浇铸完毕,一次浇铸经历5min,钢包203减重160kg/min。2) The molten stainless steel 4 metal is cast into the pouring trolley 2 through the ladle 203, and the pouring trolley 2 starts to reciprocate at 60mm/s. Molten stainless steel 4 covers the bottom of the entire metal box 3; then borax 6 is loaded into the pouring trolley 2 and spread on the surface of the stainless steel 4 by the mobility of the trolley. The two casting processes ensure that the speed of the pouring trolley 2 is consistent, so that the stainless steel 4 After the liquid falls, it will be covered by the protective agent before oxidation occurs; finally, the pouring trolley 2 casts 800kg of the 1600°C high-temperature carbon steel 7 metal liquid onto the protective agent; When the protective gas is passed, the two kinds of molten steel will be covered with protective gas and protective sand before being oxidized by oxygen after falling, effectively preventing the molten steel from being oxidized instantly due to high temperature; the casting speed of the pouring trolley 2 is kept at 50-70mm/s. The molten steel will be casted once the trolley moves in one direction, and the casting time is 5 minutes, and the weight of the ladle 203 is reduced by 160kg/min.
3)在保护气体环境下,钢液会在小车单方向移动一次就浇铸完毕。一次浇铸经历5min,钢包203减重160kg/min。两种钢液浇铸完成后,利用高压气除去保护砂及氧化杂质,最后经冷却结晶得到复合钢板。制成的铸锭尺寸为2000×8000×2000mm,经抛光观测两种相的复合界面发现其平直稳定,界面处无氧化和夹杂,结合良好。3) Under the protective gas environment, the molten steel will move in one direction on the trolley once and then the casting will be completed. A casting time takes 5 minutes, and the ladle 203 loses weight by 160kg/min. After the casting of the two molten steels is completed, the protective sand and oxidized impurities are removed by high-pressure gas, and finally the composite steel plate is obtained through cooling and crystallization. The size of the produced ingot is 2000×8000×2000mm. After polishing and observing the composite interface of the two phases, it is found that it is straight and stable, there is no oxidation and inclusions at the interface, and the combination is good.
实施例2Example 2
见图1,复合板坯铸造方法,包括以下步骤:See Fig. 1, composite slab casting method, comprises the following steps:
1)将待复合的两种金属分别熔炼,然后精炼,将获得的两种合金液(不锈钢4液和其它钢液)分别静置。保证电动机1的功率为120kW以上,浇注小车2开始以60mm/s进行往复移动,先铺满一层熔融态的不锈钢4,进而铺满一层硼砂6,最后利用钢包203将制得的其他钢液铸入小车中。此时所加钢液的质量为1000kg,处于钢包203中的钢液从上往下进行浇铸。底部箱体3,其尺寸为2000×8000×2000mm,钢液落下后来不及被氧气氧化就会被保护气和保护砂覆盖笼罩,有效防止钢液由于高温而被瞬间氧化。单种钢液会在小车单方向移动一次就浇铸完毕。一次浇铸经历3~5min,钢包203减重200kg/min。通常情况下上层钢液浇注速度要慢于底层钢液。1) The two metals to be compounded are smelted separately, and then refined, and the two obtained alloy liquids (stainless steel 4 liquid and other steel liquids) are left to stand separately. Ensure that the power of the motor 1 is above 120kW, and the pouring trolley 2 starts to reciprocate at 60mm/s, first covering a layer of molten stainless steel 4, and then covering a layer of borax 6, and finally using the ladle 203 to pour the other steel The liquid is cast into the trolley. At this time, the mass of the added molten steel is 1000kg, and the molten steel in the ladle 203 is cast from top to bottom. The bottom box 3 has a size of 2000×8000×2000 mm. After the molten steel falls, it will be covered with protective gas and protective sand before it is oxidized by oxygen, effectively preventing the molten steel from being oxidized instantly due to high temperature. A single molten steel will be casted once the trolley moves in one direction. A casting takes 3-5 minutes, and the ladle 203 loses weight by 200kg/min. Usually, the pouring speed of the upper layer of molten steel is slower than that of the bottom layer of molten steel.
2)两种钢液浇铸完成后,利用高压气除去保护砂及氧化杂质,最后经冷却结晶得到复合钢板。2) After the casting of the two molten steels is completed, the protective sand and oxidized impurities are removed by high-pressure gas, and finally the composite steel plate is obtained by cooling and crystallization.
制成的铸锭尺寸为2000×8000×2000mm,经抛光观测两种相的复合界面发现其平直稳定,界面处结合良好。The size of the produced ingot is 2000×8000×2000mm. After polishing and observing the composite interface of the two phases, it is found that it is straight and stable, and the interface is well bonded.
实施例3Example 3
见图2,复合板坯包括作为基层的Q235钢液,以及作为覆层的306钢液,两种钢液的比例应满足1:1,其厚度的取值范围为100~200mm。Q235碳钢/306不锈钢复合板坯铸造方法,包括以下步骤:As shown in Figure 2, the composite slab includes Q235 molten steel as the base layer and 306 molten steel as the cladding layer. The ratio of the two molten steels should meet 1:1, and the range of thickness is 100-200mm. Q235 carbon steel/306 stainless steel composite slab casting method, comprises the following steps:
1、利用机械臂将制得的1600℃高温的Q235钢液注入钢包203中,打开电动机开关,浇注小车2开始以50mm/s进行往复移动,所加钢液的质量为800kg,此时,旋开底部中间包207活塞,打开底部的两个承液口,处于钢包203中的钢液顺着承液管206从上往下进行浇铸。箱体3尺寸为1500×1000×400mm,在钢液注入箱体3的同时,箱体3四周上边缘处设有喷孔,在于移动方向相平行的两侧装有四个喷孔,每两个喷孔间距在200mm,流量保持在0.5L/s,在浇铸过程中会喷出保护气,部分保护砂也可由该喷孔喷出,并保证与浇注小车2保证同方向同速率,保证在钢液落下后来不及被氧气氧化就会被保护气和保护砂覆盖笼罩,有效防止钢液由于高温而被瞬间氧化。1. Use the mechanical arm to inject the prepared 1600°C high-temperature Q235 molten steel into the ladle 203, turn on the motor switch, and the pouring trolley 2 starts to reciprocate at 50mm/s, and the mass of the added molten steel is 800kg. At this time, the rotary The bottom tundish 207 piston is opened, and the two liquid receiving ports at the bottom are opened, and the molten steel in the ladle 203 is cast from top to bottom along the liquid receiving pipe 206 . The size of the box body 3 is 1500×1000×400mm. When the molten steel is injected into the box body 3, there are spray holes on the upper edge of the box body 3, and four spray holes are installed on both sides parallel to the moving direction. The distance between each nozzle hole is 200mm, and the flow rate is kept at 0.5L/s. During the casting process, the protective gas will be sprayed out, and part of the protective sand can also be sprayed out from the nozzle hole, and it must be guaranteed to be in the same direction and at the same rate as the pouring trolley 2. After the molten steel falls, before it is oxidized by oxygen, it will be covered with protective gas and protective sand, effectively preventing the molten steel from being oxidized instantly due to high temperature.
2、Q235钢液会在浇注小车2单方向移动一次就浇铸完毕。一次浇铸经历3~5min,钢包203减重160kg/min。306钢液的浇注过程和Q235钢液类似。在Q235钢液浇注完成后,箱体3以前进方向为轴向进行一定角度的倾斜,让硼砂充分覆盖在Q235钢液的表面。之后进行306钢液的浇注。此时,利用机械臂将制得的1600℃高温的306钢液注入钢包203中。重新开启电动机,浇注小车2会反方向以50mm/s进行移动,其余步骤与步骤1类似。2. The Q235 molten steel will be casted once the pouring trolley 2 moves in one direction. A casting takes 3 to 5 minutes, and the ladle 203 loses weight by 160kg/min. The pouring process of 306 molten steel is similar to that of Q235 molten steel. After the pouring of the Q235 molten steel is completed, the box body 3 is inclined at a certain angle with the forward direction as the axial direction, so that the borax is fully covered on the surface of the Q235 molten steel. After that, pouring of 306 molten steel is carried out. At this time, the prepared 306 molten steel with a high temperature of 1600° C. is injected into the ladle 203 by using a mechanical arm. Turn on the motor again, and the pouring trolley 2 will move in the opposite direction at 50mm/s, and the rest of the steps are similar to step 1.
3、两种钢液浇铸完成后,利用高压气除去保护砂及氧化杂志,最后经冷却结晶得到复合钢板。3. After the casting of the two molten steels is completed, the protective sand and oxidized impurities are removed by high-pressure gas, and finally the composite steel plate is obtained through cooling and crystallization.
本发明通过装置内模具小孔喷出的保护气和保护砂,可以构成致密的保护气氛而且保护砂由于覆盖在Q235钢液表面,可以有效排除氧气对高温金属的氧化影响。此外,由于浇铸装置的可移动性,有效避免了浇注过程中“死区”的产生,保证浇注成品的内部组织更加致密均匀。In the present invention, the protective gas and protective sand sprayed from the small holes of the mold in the device can form a dense protective atmosphere, and the protective sand can effectively eliminate the oxidation effect of oxygen on high-temperature metals because the protective sand covers the surface of the Q235 molten steel. In addition, due to the mobility of the casting device, the "dead zone" during the casting process is effectively avoided, ensuring that the internal structure of the cast product is more dense and uniform.
Claims (9)