CN107858461A - A kind of online granulation and the method for collecting melting titanium carbide slag - Google Patents

A kind of online granulation and the method for collecting melting titanium carbide slag Download PDF

Info

Publication number
CN107858461A
CN107858461A CN201711241790.2A CN201711241790A CN107858461A CN 107858461 A CN107858461 A CN 107858461A CN 201711241790 A CN201711241790 A CN 201711241790A CN 107858461 A CN107858461 A CN 107858461A
Authority
CN
China
Prior art keywords
slag
water
titanium carbide
carbide slag
melting titanium
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201711241790.2A
Other languages
Chinese (zh)
Other versions
CN107858461B (en
Inventor
王唐林
程晓哲
黄家旭
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Pangang Group Panzhihua Iron and Steel Research Institute Co Ltd
Original Assignee
Pangang Group Panzhihua Iron and Steel Research Institute Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Pangang Group Panzhihua Iron and Steel Research Institute Co Ltd filed Critical Pangang Group Panzhihua Iron and Steel Research Institute Co Ltd
Priority to CN201711241790.2A priority Critical patent/CN107858461B/en
Publication of CN107858461A publication Critical patent/CN107858461A/en
Application granted granted Critical
Publication of CN107858461B publication Critical patent/CN107858461B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention belongs to high-temperature metallurgical slag to be granulated field, and in particular to a kind of online granulation and the method for collecting melting titanium carbide slag.The technical problems to be solved by the invention are to provide a kind of online granulation and the method for collecting melting titanium carbide slag; using water to its continuous injection while fire door is flowed out into melting titanium carbide slag process; it is 0.3~0.4MPa to control delivery port pressure; distance is 0.8~1.2m; slag-water slurry falls into slag pond; substantial amounts of water in slag-water slurry is removed, slag is collected after drying.The inventive method is simple to operate, cost is low, and gained slag particle degree is respectively less than 3mm.

Description

一种在线粒化及收集熔融碳化钛渣的方法A method for in-line granulation and collection of molten titanium carbide slag

技术领域technical field

本发明涉及高温冶金渣粒化领域,具体涉及一种在线粒化及收集熔融碳化钛渣的方法。The invention relates to the field of high-temperature metallurgical slag granulation, in particular to a method for granulating and collecting molten titanium carbide slag.

背景技术Background technique

攀西地区钒钛磁铁矿经高炉冶炼后,产生含TiO222%左右的高钛型高炉渣,随着高炉渣的排放,其中的钛资源也被堆放或者流失,造成了大量宝贵资源浪费。因此,从高钛型高炉渣中对钛进行分离提取成为攀西钒钛磁铁矿资源综合利用的重要途径。After the vanadium-titanium magnetite in Panxi area is smelted in the blast furnace, high-titanium blast furnace slag containing about 22% TiO 2 is produced. With the discharge of blast furnace slag, the titanium resources in it are also piled up or lost, resulting in a lot of waste of valuable resources. . Therefore, the separation and extraction of titanium from high-titanium blast furnace slag has become an important way for the comprehensive utilization of vanadium-titanium magnetite resources in Panxi.

近年来,通过对高钛型高炉渣的不断研究,高温碳化—低温氯化工艺以其流程短、处理量大、提钛率高等优势得到了推广和应用。该工艺首先将高钛型高炉渣在1550℃以上的高温条件下用碳质还原剂还原成TiC,出炉冷却后将其破磨至80~200目供低温氯化制备TiCl4,精制后成为钛白粉或海绵钛的生产原料。In recent years, through continuous research on high-titanium blast furnace slag, the high-temperature carbonization-low-temperature chlorination process has been promoted and applied due to its advantages of short process, large processing capacity, and high titanium extraction rate. In this process, the high-titanium blast furnace slag is first reduced to TiC with a carbonaceous reducing agent at a high temperature above 1550°C, and after being cooled, it is broken and ground to 80-200 mesh for low-temperature chlorination to prepare TiCl 4 , which is refined into titanium Raw material for the production of white powder or titanium sponge.

高炉渣经高温碳化形成碳化渣以后,需破磨后才能满足低温氯化的使用,因此,如何实现碳化渣高效、经济的破磨处理技术,是衔接高温碳化—低温氯化工艺的关键环节。采用传统的渣盘接渣,空冷后再破磨处理技术,碳化渣需经过冲击破碎—颚式破碎—球磨等一系列高能耗处理方式才能达到要求,不仅使得处理流程长、劳动强度大,而且处理的成本也非常高。After the blast furnace slag is carbonized at high temperature to form carbonized slag, it needs to be crushed and ground to meet the use of low-temperature chlorination. Therefore, how to realize the efficient and economical crushing and grinding treatment technology of carbide slag is a key link in the connection between high-temperature carbonization and low-temperature chlorination process. The traditional technology of slag receiving from the slag tray, crushing and grinding after air cooling, the carbonized slag needs to go through a series of high-energy-consuming treatment methods such as impact crushing-jaw crushing-ball milling to meet the requirements, not only makes the processing process long and labor-intensive, but also The cost of processing is also very high.

发明内容Contents of the invention

为了改善传统破磨碳化渣工艺技术的不足,本发明提供一种在线粒化及收集熔融碳化钛渣的方法。该方法在碳化钛渣出渣过程中采用高压水柱对液态渣进行强制冲击冷却,经冲散冷却后的碳化渣和冲渣水落入沉渣池中,沉渣池中的水经滤网流入沉淀池后再溢流进入澄清池,在澄清池外接水源补水,作为冲渣水循环使用;再用吸渣泵将水淬后的渣连续输送至堆渣场,待其风干或烘干后供低温氯化使用。该处理技术流程短、成本低、且极大地改善了现场工作环境,为高炉渣高温碳化—低温氯化提供了一条经济环保的工艺技术路线。In order to improve the deficiencies of the traditional technology of grinding carbide slag, the present invention provides a method for granulating and collecting molten titanium carbide slag. In this method, high-pressure water column is used to forcibly impinge and cool the liquid slag during the slag removal process of titanium carbide slag, and the carbide slag and slag flushing water after being washed away and cooled fall into the sedimentation tank, and the water in the sedimentation tank flows into the sedimentation tank through the filter screen. Then it overflows into the clarification tank, and the outside of the clarification tank is connected with a water source to make up water, which is recycled as slag flushing water; the water-quenched slag is continuously transported to the slag dump by the slag suction pump, and it is used for low-temperature chlorination after it is air-dried or dried use. The treatment technology has a short process, low cost, and greatly improves the working environment on site, and provides an economical and environmentally friendly process technology route for high-temperature carbonization-low-temperature chlorination of blast furnace slag.

本发明所要解决的技术问题是提供一种在线粒化及收集熔融碳化钛渣的方法。该方法包括以下步骤:碳化结束后,炉口流出熔融碳化钛渣过程的同时采用水对其连续喷射,控制出水口压力为0.3~0.4MPa,熔融碳化钛渣与出水口的垂直距离为0.8~1.2m,渣水混合物落入沉渣池,除去渣水混合物中的水,水淬渣经干燥后收集即可。The technical problem to be solved by the present invention is to provide a method for granulating and collecting molten titanium carbide slag. The method includes the following steps: after the carbonization is completed, water is continuously sprayed on the molten titanium carbide slag during the process of flowing out from the furnace mouth, the pressure of the water outlet is controlled to be 0.3-0.4 MPa, and the vertical distance between the molten titanium carbide slag and the water outlet is 0.8-0.8 MPa. 1.2m, the slag-water mixture falls into the sedimentation tank, the water in the slag-water mixture is removed, and the water-quenched slag is dried and collected.

进一步的,上述在线粒化及收集熔融碳化钛渣的方法,包括以下步骤:碳化结束后,炉口流出熔融碳化钛渣过程的同时采用水对其连续喷射,控制出水口压力为0.3~0.4MPa,熔融碳化钛渣与出水口的垂直距离为0.8~1.2m,渣水混合物落入沉渣池,沉渣池中的水经滤网隔离流入沉淀池,再溢流进入澄清池;沉渣池内的水淬渣经吸渣泵连续输送至堆渣场,水淬渣经干燥后收集即可。Further, the above-mentioned method for granulating and collecting molten titanium carbide slag includes the following steps: after the carbonization is completed, water is continuously sprayed on it while the molten titanium carbide slag flows out of the furnace mouth, and the pressure at the water outlet is controlled to be 0.3-0.4 MPa , the vertical distance between the molten titanium carbide slag and the water outlet is 0.8-1.2m, the slag-water mixture falls into the sedimentation tank, the water in the sedimentation tank flows into the sedimentation tank through filter screen isolation, and then overflows into the clarification tank; the water quenching in the sedimentation tank The slag is continuously transported to the slag dump by the slag suction pump, and the water-quenched slag can be collected after being dried.

优选的,上述在线粒化及收集熔融碳化钛渣的方法中,控制熔融碳化钛渣与水的重量比为1︰8~10。Preferably, in the above method of granulating and collecting molten titanium carbide slag, the weight ratio of molten titanium carbide slag to water is controlled to be 1:8-10.

优选的,上述在线粒化及收集熔融碳化钛渣的方法中,出水口的宽度≥流出的熔融碳化钛渣的宽度。Preferably, in the above-mentioned method for granulating and collecting molten titanium carbide slag, the width of the water outlet ≥ the width of the outflowing molten titanium carbide slag.

进一步的,上述在线粒化及收集熔融碳化钛渣的方法中,通过将出水口分为多个格子来控制出水口的宽度,所述的多个为2个以上。Further, in the above-mentioned method for granulating and collecting molten titanium carbide slag, the width of the water outlet is controlled by dividing the water outlet into a plurality of grids, and the plurality of grids is more than two.

优选的,上述在线粒化及收集熔融碳化钛渣的方法中,所述沉渣池的深度为5~7m。Preferably, in the method for granulating and collecting molten titanium carbide slag, the depth of the sediment pool is 5-7m.

优选的,上述在线粒化及收集熔融碳化钛渣的方法中,控制干燥后的水淬渣的含水量为15~20%。Preferably, in the above-mentioned method for granulating and collecting molten titanium carbide slag, the water content of the dried water-quenched slag is controlled to be 15-20%.

本发明方法采用高压高速水对冶炼结束后流程的熔融碳化钛渣进行喷射,控制合适的水量和压力等参数,不需外加磨矿等手段,即可获得粒度均小于3mm的碳化钛渣,满足后续使用要求。本发明处理技术流程短、成本低、且极大地改善了现场工作环境,为高炉渣高温碳化—低温氯化提供了一条经济环保的工艺技术路线。The method of the present invention uses high-pressure and high-speed water to spray the molten titanium carbide slag in the process after the smelting process, controls parameters such as suitable water volume and pressure, and can obtain titanium carbide slag with a particle size of less than 3 mm without additional means such as grinding ore, which meets the requirements Subsequent use requirements. The invention has short processing technical process, low cost and greatly improves the on-site working environment, and provides an economical and environment-friendly technological route for high-temperature carbonization-low-temperature chlorination of blast furnace slag.

具体实施方式Detailed ways

本发明提供了一种处理熔融碳化钛渣的方法,包括以下步骤:采用水淬方式,借助连续喷射出的高压高速水流瞬间击散并冷却熔融碳化钛渣,控制出水口压力为0.3~0.4MPa,熔融碳化钛渣与出水口的垂直距离为0.8~1.2m,使其粒化形成小颗粒渣,与冲渣水形成渣水混合物进入沉渣池;沉渣池中的水经滤网流入沉淀池后再溢流进入澄清池,在澄清池外接水源补水,作为冲渣水循环使用;沉渣池内的水淬渣经吸渣泵连续输送至堆渣场,经电炉烟气余热或其它方式烘干并控制其水分含量,以避免运输过程扬尘同时保证立磨入料要求;另随水淬渣一起输送至堆渣场的水经排水孔回流至接渣池作为循环水使用。采用该技术方案,可极大缩短碳化渣破磨流程、节省破磨成本并改善工作环境。The invention provides a method for processing molten titanium carbide slag, which includes the following steps: adopting water quenching method to instantly break up and cool the molten titanium carbide slag with the help of continuously sprayed high-pressure and high-speed water flow, and controlling the water outlet pressure to be 0.3-0.4 MPa , the vertical distance between the molten titanium carbide slag and the water outlet is 0.8-1.2m, making it granulated to form small particle slag, which forms a slag-water mixture with the slag flushing water and enters the sedimentation tank; the water in the sedimentation tank flows into the sedimentation tank through the filter screen Then it overflows into the clarification tank, and the outside of the clarification tank is connected with a water source to make up water, which is recycled as slag washing water; the water-quenched slag in the sediment tank is continuously transported to the slag dump by the slag suction pump, dried by the waste heat of the electric furnace flue gas or other methods and controlled. Moisture content, in order to avoid dust during transportation and ensure the requirements of vertical mill feeding; in addition, the water transported to the slag yard along with the water-quenched slag is returned to the slag receiving pool through the drainage hole for use as circulating water. Adopting this technical solution can greatly shorten the grinding process of carbide slag, save grinding costs and improve the working environment.

优选的,上述方法采用高压水枪进行水淬,借助连续喷射出的高压高速水流瞬间击散并冷却熔融碳化钛渣,使其粒化形成小颗粒渣。Preferably, the above method uses a high-pressure water gun for water quenching, and the molten titanium carbide slag is instantly dispersed and cooled by the continuously sprayed high-pressure and high-speed water flow, so that it is granulated to form small particle slag.

进一步的,通过采用对出水口分成多个小格的方式来控制水宽与熔融碳化钛渣宽相匹配,保证一次性将所有熔融钛渣水淬完全。水流在喷嘴处因吸卷和重力作用,呈喇叭状向外扩散,并形成高速密集水幕,保证熔融渣流伸入水幕。Further, by dividing the water outlet into a plurality of small cells to control the matching of the width of the water with the width of the molten titanium carbide slag, it is ensured that all the molten titanium slag is fully water-quenched at one time. Due to suction and gravity, the water flow spreads outward in the shape of a trumpet at the nozzle, and forms a high-speed dense water curtain to ensure that the molten slag flows into the water curtain.

进一步的,出水口的水压为0.3~0.4MPa,形成高压高速水幕,同时利用水幕内各点速度差及内摩擦力将流入其内的熔融渣瞬间击散并冷却,保证其粒度均小于3mm,与冲渣水形成渣水混合物进入沉渣池。Further, the water pressure at the water outlet is 0.3-0.4 MPa to form a high-pressure and high-speed water curtain, and at the same time, the molten slag flowing into it is instantly broken up and cooled by using the speed difference and internal friction of each point in the water curtain to ensure that its particle size is less than 3mm, form a slag-water mixture with flushing slag water and enter the sedimentation tank.

进一步的,所述渣水比为1︰8~10,以确保带走渣水瞬间接触产生的热量。Further, the slag-water ratio is 1:8-10 to ensure that the heat generated by the instant contact of slag-water is taken away.

进一步的,所述沉渣池深度5~7米以保证能充分容纳渣水混合物,同时防止形成渣裹水造成爆炸的危险。Further, the depth of the sediment pool is 5-7 meters to ensure that the mixture of slag and water can be fully accommodated, and at the same time, the risk of explosion caused by the formation of slag-wrapped water is prevented.

进一步的,所述沉淀池与沉渣池之间采用滤网隔离,保证水淬后渣不进入沉淀池,同时沉淀池与澄清池采用高位挡墙隔离,沉淀池中的水经充分沉淀后溢流进入澄清池,作为循环冲渣水使用。Further, the sedimentation tank and the sedimentation tank are separated by a filter to ensure that the slag does not enter the sedimentation tank after water quenching. At the same time, the sedimentation tank and the clarification tank are separated by a high retaining wall, and the water in the sedimentation tank overflows into the sedimentation tank after being fully settled. The clarifier is used as circulating slag flushing water.

进一步的,所述澄清池一方面利用沉淀池溢流进入的水进行补给,另一方面外接工业用水,以确保充足的冲渣水源。Further, on the one hand, the clarification tank is replenished with the water overflowed from the sedimentation tank, and on the other hand, it is connected with industrial water to ensure sufficient slag washing water source.

进一步的,所述水淬渣采用吸渣泵将沉淀池中的渣水混合物连续输送至临时堆渣场,利用电炉烟气余热烘干并控制水淬渣水分含量为15~20%,以避免运输过程扬尘同时保证水淬渣立磨入料要求。Further, the water-quenched slag uses a slag suction pump to continuously transport the slag-water mixture in the sedimentation tank to a temporary slag dump, uses the waste heat of the electric furnace flue gas to dry and controls the water-quenched slag moisture content to 15-20%, so as to avoid During the transportation process, the dust is raised while ensuring the feeding requirements of the water-quenched slag vertical mill.

进一步的,所述渣水混合物,经吸渣泵输送至临时堆渣场后,水经排水孔回流至接渣池作为循环水使用。Further, after the slag-water mixture is transported to the temporary slag dump by the slag suction pump, the water flows back to the slag receiving pool through the drain hole for use as circulating water.

下面对本发明的具体实施方式作详细说明。需要指出的是此处所作的具体实施方式仅用于说明和解释本发明,并不用于限制本发明。Specific embodiments of the present invention will be described in detail below. It should be pointed out that the specific implementation methods here are only used to illustrate and explain the present invention, and are not intended to limit the present invention.

实施例一种在线粒化及收集熔融碳化钛渣的方法Embodiment A kind of method of in-line graining and collecting molten titanium carbide slag

待碳化电炉冶炼接近终点时,打开水泵及吸渣泵,控制压力为0.3~0.4MPa,形成高压高速水幕后开炉口,使炉内的高温熔融碳化渣在静压力作用下流入水幕,此时调整渣水比至1:8~10,熔融碳化渣在水幕内被瞬间击散并冷凝成小颗粒渣进入沉渣池,而后被吸渣泵输送至临时堆渣场。同时沉渣池内的水经格网进入沉淀池,再经溢流进入澄清池,随水淬渣一同输送至临时堆渣场的水经排水口反流至沉渣池。When the smelting of the carbonization electric furnace is close to the end, turn on the water pump and the slag suction pump, control the pressure at 0.3-0.4MPa, form a high-pressure and high-speed water curtain and open the furnace opening, so that the high-temperature molten carbide slag in the furnace flows into the water curtain under the action of static pressure. Adjust the ratio of slag to water to 1:8~10, the molten carbide slag is instantly dispersed in the water curtain and condensed into small particle slag, which enters the sedimentation tank, and then is transported to the temporary slag dump by the slag suction pump. At the same time, the water in the sedimentation tank enters the sedimentation tank through the grid, and then enters the clarification tank through the overflow, and the water that is transported to the temporary slag dump together with the water-quenched slag flows back to the sedimentation tank through the outlet.

经烟气烘干后的水淬碳化钛渣,其含水量为15-20%,粒度全部在3mm以下。使用该水淬碳化钛渣可使吨渣破磨成本降低70元,80~200目碳化钛成品渣提高约20%,极大地降低了碳化渣破磨成本。The water-quenched titanium carbide slag dried by flue gas has a water content of 15-20% and a particle size of less than 3mm. The use of the water-quenched titanium carbide slag can reduce the cost of crushing and grinding per ton of slag by 70 yuan, and increase the finished slag of 80-200 mesh titanium carbide by about 20%, which greatly reduces the cost of grinding and grinding the carbide slag.

以上内容详细描述了本发明的设计原则以及应用实施方式,但是,本发明并不限于上述实施方式中的具体细节,在本发明的技术构思范围内,可以对本发明的技术方案进行多种简单变型,这些简单变型均属于本发明的保护范围。The above content has described the design principle and application implementation of the present invention in detail, but the present invention is not limited to the specific details in the above-mentioned implementation, and within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention , these simple modifications all belong to the protection scope of the present invention.

Claims (7)

1. online granulation and the method for collecting melting titanium carbide slag, it is characterised in that:Comprise the following steps:After carbonization terminates, stove Using water to its continuous injection while mouth outflow melting titanium carbide slag process, it is 0.3~0.4MPa to control delivery port pressure, is melted The vertical range for melting titanium carbide slag and delivery port is 0.8~1.2m, and slag-water slurry falls into detritus tank, removes in slag-water slurry Water, Water Quenching Slag collects after drying.
2. online granulation according to claim 1 and the method for collecting melting titanium carbide slag, it is characterised in that:Including following Step:After carbonization terminates, delivery port pressure is controlled to its continuous injection using water while fire door outflow melts titanium carbide slag process Power is 0.3~0.4MPa, and the vertical range for melting titanium carbide slag and delivery port is 0.8~1.2m, and slag-water slurry falls into sediment Pond, the water in detritus tank is isolated through filter screen flows into sedimentation basin, then overflow enters depositing reservoir;Water Quenching Slag in detritus tank is through Residue suction pump Continuous conveying is collected to slag tip after drying.
3. online granulation according to claim 1 or 2 and the method for collecting melting titanium carbide slag, it is characterised in that:Control The weight ratio for melting titanium carbide slag and water is 1 ︰ 8~10.
4. online granulation according to claim 1 or 2 and the method for collecting melting titanium carbide slag, it is characterised in that:Water outlet The width of the melting titanium carbide slag of width >=outflow of mouth.
5. online granulation according to claim 4 and the method for collecting melting titanium carbide slag, it is characterised in that:By that will go out The mouth of a river is divided into multiple grid to control the width of delivery port, it is described it is multiple be more than 2.
6. online granulation according to claim 1 or 2 and the method for collecting melting titanium carbide slag, it is characterised in that:It is described The depth of detritus tank is 5~7m.
7. the method for the online granulation and collection melting titanium carbide slag according to any one of claim 1~6, its feature exist In:The water content for controlling dried Water Quenching Slag is 15~20%.
CN201711241790.2A 2017-11-30 2017-11-30 Method for online granulating and collecting molten titanium carbide slag Active CN107858461B (en)