CN106555205A - 一种离子膜电解槽阳极网的清洗方法 - Google Patents

一种离子膜电解槽阳极网的清洗方法 Download PDF

Info

Publication number
CN106555205A
CN106555205A CN201611091608.5A CN201611091608A CN106555205A CN 106555205 A CN106555205 A CN 106555205A CN 201611091608 A CN201611091608 A CN 201611091608A CN 106555205 A CN106555205 A CN 106555205A
Authority
CN
China
Prior art keywords
pure water
cleaning agent
cleaning
anode
ion
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201611091608.5A
Other languages
English (en)
Inventor
陈映志
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
PANZIHUA STEEL XINYU CHEMICAL CO Ltd
Original Assignee
PANZIHUA STEEL XINYU CHEMICAL CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by PANZIHUA STEEL XINYU CHEMICAL CO Ltd filed Critical PANZIHUA STEEL XINYU CHEMICAL CO Ltd
Priority to CN201611091608.5A priority Critical patent/CN106555205A/zh
Publication of CN106555205A publication Critical patent/CN106555205A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种离子膜电解槽阳极网的清洗方法,能有效去除阳极网表面的化合物垢层、避免阳极网的表面涂层被破坏,从而降低电解槽电压。包括如下步骤:用纯水对清洗槽进行预清洗和试漏,用塑料薄膜间隔压紧电解槽的阴阳极后放入清洗槽中;用纯水配制一次清洗剂,一次清洗剂中其它成分按浓度百分比计为:盐酸2%~6%、lan‑826缓蚀剂0.2%~0.3%,将一次清洗剂加热至55~85℃后对电解槽阳极网清洗1~4h,再排尽一次清洗液,加入纯水冲洗;用纯水配制二次清洗剂,二次清洗剂中其它成分按浓度百分比计为:柠檬酸3%~8%、lan‑826缓蚀剂0.2%~0.35%、氨基磺酸钠3%~6%,将二次清洗剂加热至55~85℃后对电解槽阳极网清洗4~6h,再排尽二次清洗液,加入纯水冲洗。

Description

一种离子膜电解槽阳极网的清洗方法
技术领域
本发明涉及氯碱化工领域,尤其是一种离子膜电解槽阳极网的清洗方法。
背景技术
离子膜电解槽在生产过程中,阳极网长期与精盐水接触,氯碱行业中精盐水的铁含量长期大于20ppm,精盐水中还存在一定量的钙、镁,经过长时间的生产后,阳极网的表面会沉淀大量铁、钙、镁化合物,破坏阳极网的表面涂层并形成垢层,而阳极网产生垢层会使离子膜老化,从而造成电解槽电压升高、电流效率下降、生产电耗大幅增加。
发明内容
本发明所要解决的技术问题是:提供一种离子膜电解槽阳极网的清洗方法,能有效去除阳极网表面的化合物垢层、避免阳极网的表面涂层被破坏,从而降低电解槽电压。
为解决上述技术问题本发明所采用的技术方案是:一种离子膜电解槽阳极网的清洗方法,包括如下步骤:
a、用纯水对清洗槽进行预清洗和试漏,用塑料薄膜间隔压紧电解槽的阴阳极后放入清洗槽中;
b、用纯水配制一次清洗剂,一次清洗剂中其它成分按浓度百分比计为:盐酸2%~6%、lan-826缓蚀剂0.2%~0.3%,将一次清洗剂加热至55~85℃后对电解槽阳极网清洗1~4h,再排尽一次清洗液,加入纯水冲洗;
c、用纯水配制二次清洗剂,二次清洗剂中其它成分按浓度百分比计为:柠檬酸3%~8%、lan-826缓蚀剂0.2%~0.35%、氨基磺酸钠3%~6%,将二次清洗剂加热至55~85℃后对电解槽阳极网清洗4~6h,再排尽二次清洗液,加入纯水冲洗。
进一步的是:步骤b中对一次清洗剂的加热、步骤c中对二次清洗剂的加热都采用通蒸汽进行加热。
进一步的是:步骤b中加入纯水冲洗至少2次。
进一步的是:步骤c中加入纯水冲洗至少3次。
本发明的有益效果是:
1、一次清洗剂对铁、钙、镁化合物的溶解能力强,可有效溶解阳极网的垢层,对降低电解槽电压的效果显著;
2、lan-826缓蚀剂能降低一次清洗剂的溶解速率,可避免一次清洗剂局部反应过快而破坏阳极网的表面涂层;
3、二次清洗剂溶解过程的反应速率不快,与阳极网涂层的反应几率小,对涂层的影响小;
4、本发明兼顾对阳极网的清洗和对阳极网表面涂层的保护,有效溶解阳极网垢层的同时不会对表面涂层产生破坏,不会影响阳极网的原有功能。
具体实施方式
为了便于理解本发明,下面结合实施例对本发明进行进一步的说明。
本发明一种离子膜电解槽阳极网的清洗方法包括如下步骤:
a、用纯水对清洗槽进行预清洗和试漏,用塑料薄膜间隔压紧电解槽的阴阳极后放入清洗槽中;
b、用纯水配制一次清洗剂,一次清洗剂中其它成分按浓度百分比计为:盐酸2%~6%、lan-826缓蚀剂0.2%~0.3%,将一次清洗剂加热至55~85℃后对电解槽阳极网清洗1~4h,再排尽一次清洗液,加入纯水冲洗;
c、用纯水配制二次清洗剂,二次清洗剂中其它成分按浓度百分比计为:柠檬酸3%~8%、lan-826缓蚀剂0.2%~0.35%、氨基磺酸钠3%~6%,将二次清洗剂加热至55~85℃后对电解槽阳极网清洗4~6h,再排尽二次清洗液,加入纯水冲洗。
步骤b中对一次清洗剂的加热、步骤c中对二次清洗剂的加热都采用通蒸汽进行加热。
步骤b中加入纯水冲洗至少2次。
步骤c中加入纯水冲洗至少3次。
实施例
取待大修的电解槽阳极网,同区域的阳极网裁剪成三等份后做成3中样本进行浸泡处理,样1不做清洗处理、样2直接用纯水进行清洗处理、样3按本发明的清洗步骤进行清洗处理,清洗完成后通过仪器扫描各样本的表层成分含量,结果如下:
名称 Ru Ir Fe
样1 1.44 4.73 18.42
样2 1.45 4.73 16.34
样3 1.42 4.72 3.25
由表中可知,按本发明的要求进行清理处理的电解槽阳极网,表面所含的Fe含量大大降低,而Ru、Ir为阳极网表面涂层的成分,两者含量跟未经清洗处理的样1中的含量相差甚微,说明本发明的清洗过程只会溶解垢层而不会对阳极网的表面涂层产生影响。
清洗前对样3的电解槽单槽电压测试为3.12V,清洗后样3的电解槽单槽电压为2.95V,单槽的电压下降0.17V。

Claims (4)

1.一种离子膜电解槽阳极网的清洗方法,其特征在于:包括如下步骤:
a、用纯水对清洗槽进行预清洗和试漏,用塑料薄膜间隔压紧电解槽的阴阳极后放入清洗槽中;
b、用纯水配制一次清洗剂,一次清洗剂中其它成分按浓度百分比计为:盐酸2%~6%、lan-826缓蚀剂0.2%~0.3%,将一次清洗剂加热至55~85℃后对电解槽阳极网清洗1~4h,再排尽一次清洗液,加入纯水冲洗;
c、用纯水配制二次清洗剂,二次清洗剂中其它成分按浓度百分比计为:柠檬酸3%~8%、lan-826缓蚀剂0.2%~0.35%、氨基磺酸钠3%~6%,将二次清洗剂加热至55~85℃后对电解槽阳极网清洗4~6h,再排尽二次清洗液,加入纯水冲洗。
2.如权利要求1所述的一种离子膜电解槽阳极网的清洗方法,其特征在于:步骤b中对一次清洗剂的加热、步骤c中对二次清洗剂的加热都采用通蒸汽进行加热。
3.如权利要求1所述的一种离子膜电解槽阳极网的清洗方法,其特征在于:步骤b中加入纯水冲洗至少2次。
4.如权利要求1所述的一种离子膜电解槽阳极网的清洗方法,其特征在于:步骤c中加入纯水冲洗至少3次。
CN201611091608.5A 2016-12-01 2016-12-01 一种离子膜电解槽阳极网的清洗方法 Pending CN106555205A (zh)