CN106198288A - The method of inspection of a kind of coated layer adhesion and verifying attachment - Google Patents
The method of inspection of a kind of coated layer adhesion and verifying attachment Download PDFInfo
- Publication number
- CN106198288A CN106198288A CN201610710687.7A CN201610710687A CN106198288A CN 106198288 A CN106198288 A CN 106198288A CN 201610710687 A CN201610710687 A CN 201610710687A CN 106198288 A CN106198288 A CN 106198288A
- Authority
- CN
- China
- Prior art keywords
- grinding
- coating
- drum
- outer cylinder
- bearing
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明公开了一种涂镀层结合力的检验方法以及检验装置,其中,检验方法包括:将待检的涂镀层零件放入放置有预定数量磨球的滚筒中;将滚筒浸在预定体积、预定温度的研磨液中;设置滚筒转速、研磨时间,并进行预定时间的研磨;检查零件涂镀层是否存在起泡、脱落现象,其中,滚筒的侧壁设置有多个小孔,所述小孔的直径小于磨球的直径;若是,判定涂镀层不合格,若否,判定涂镀层合格。所述涂镀层结合力的检验方法以及检验装置,原理简单、操作方便,与已有的热震法、划格法、胶粘法相比,能够实现快捷有效且百分之百的零件检验,还可根据待检零件材质选择不同的磨球和研磨液,设置研磨参数提供多种工作模式,实现不同零件涂镀层结合力的最优检验。
The invention discloses an inspection method and an inspection device for coating binding force, wherein the inspection method includes: putting a coated part to be inspected into a drum with a predetermined number of grinding balls; immersing the drum in a predetermined volume, a predetermined temperature; set the drum speed, grinding time, and grind for a predetermined time; check whether there is foaming or shedding in the coating of the part, wherein the side wall of the drum is provided with a plurality of small holes, and the holes The diameter is smaller than the diameter of the grinding ball; if it is, it is judged that the coating is unqualified, if not, it is judged that the coating is qualified. The inspection method and inspection device for the bonding force of the coating layer are simple in principle and convenient in operation. Different grinding balls and grinding liquids are selected for the material of the inspection parts, and the grinding parameters are set to provide a variety of working modes to achieve the optimal inspection of the coating bonding force of different parts.
Description
技术领域technical field
本发明涉及涂镀领域,具体涉及一种涂镀层结合力的检验方法及检验装置。The invention relates to the field of coating, in particular to a testing method and testing device for the binding force of the coating.
背景技术Background technique
涂镀层有抗氧化性、耐磨性、耐腐蚀性等性能,广泛地应用于工业的各个领域。基体材料与其表面涂镀层间的结合力是表征涂镀层质量的重要指标,好的结合力是金属涂镀层发挥性能的重要因素。The coating has oxidation resistance, wear resistance, corrosion resistance and other properties, and is widely used in various fields of industry. The bonding force between the base material and the surface coating is an important index to characterize the quality of the coating, and a good bonding force is an important factor for the performance of the metal coating.
目前,根据国内现有标准和规范,工厂常用热震法、划格法和胶粘法等方法来检验涂镀层的结合力。热震法主要是利用涂镀层材料与基体材料有不同的膨胀系数,此法适合膨胀系数相差较大的涂镀层结合力检验,对于膨胀系数相近的涂镀层结合力检验效果不明显。划格法要求钢刀在涂镀层上划深度恰好达基体的方格,属于破坏性检验,不适合百分之百的零件检验。胶粘法因胶层结合强度的影响,一般与划格法配合使用。此法不适合百分之百的零件检验。At present, according to the existing domestic standards and specifications, factories often use methods such as thermal shock method, cross-cut method and adhesive method to test the bonding force of the coating. The thermal shock method mainly uses the different expansion coefficients of the coating material and the base material. This method is suitable for testing the bonding force of the coating with a large difference in expansion coefficient. The effect of testing the bonding force of the coating with a similar expansion coefficient is not obvious. The cross-hatching method requires a steel knife to scratch a square on the coating that is just deep enough to reach the substrate, which is a destructive inspection and is not suitable for 100% part inspection. The adhesive method is generally used in conjunction with the cross-cut method due to the influence of the bonding strength of the adhesive layer. This method is not suitable for 100% part inspection.
综上所述,如何提供一种涂镀层结合力检验方法及其装置,以实现快捷有效且百分之百的零件检验,是目前本领域技术人员亟待解决的问题。To sum up, how to provide a method and device for inspecting the bonding force of coatings and coatings, so as to realize fast, effective and 100% parts inspection, is an urgent problem to be solved by those skilled in the art.
发明内容Contents of the invention
本发明的目的是提供一种涂镀层结合力的检验方法及检验装置,以实现快捷有效且百分之百的零件检验,操作方便。The purpose of the present invention is to provide an inspection method and inspection device for the binding force of the coating and plating layer, so as to realize fast, effective and 100% part inspection, and the operation is convenient.
为解决上述技术问题,本发明实施例提供了一种涂镀层结合力的检验方法,包括:In order to solve the above technical problems, an embodiment of the present invention provides a method for testing the adhesion of coatings, including:
将待检的涂镀层零件放入放置有预定数量磨球的滚筒中;Put the coated parts to be inspected into the drum with a predetermined number of grinding balls;
将所述滚筒浸在预定体积、预定温度的研磨液中;immersing the drum in a predetermined volume and temperature of grinding liquid;
设置所述滚筒转速、研磨时间,并进行预定时间的研磨;Set the rotating speed and grinding time of the drum, and perform grinding for a predetermined time;
检查所述零件涂镀层是否存在起泡、脱落现象,其中,所述滚筒的侧壁设置有多个小孔,所述小孔的直径小于所述磨球的直径;Check whether there are bubbles and shedding phenomena in the coating of the part, wherein the side wall of the drum is provided with a plurality of small holes, and the diameter of the small holes is smaller than the diameter of the grinding ball;
若是,判定所述涂镀层不合格,若否,判定所述涂镀层合格。If yes, it is determined that the coating is unqualified; if not, it is determined that the coating is qualified.
其中,所述设置所述滚筒转速、研磨时间,并进行预定时间的研磨,还包括:Wherein, the setting of the rotating speed of the drum, the grinding time, and the grinding for a predetermined time also include:
对所述涂镀层零件进行超声波扫描。An ultrasonic scan is performed on the coated part.
除此之外,本发明实施例还提供了一种涂镀层结合力的检验装置,包括机体、操作面板和装料门,所述机体的内部设置有滚筒和外筒,所述滚筒壁上均匀设置多个相同孔径的小孔,所述滚筒内放置有预定数量磨球,所述外筒套接在所述滚筒的外壁上,所述外筒和所述滚筒的第一端通过第一轴承密封连接,第二端设置有用于放取零件的窗口,所述窗口与装料门密封连接;还包括设置在所述基体底部的驱动机构,所述驱动机构与所述第一轴承连接,并通过带动所述第一轴承转动带动所述滚筒转动;In addition, the embodiment of the present invention also provides an inspection device for coating bonding force, which includes a machine body, an operation panel and a charging door. A drum and an outer cylinder are arranged inside the body, and the wall of the drum is uniformly arranged A plurality of small holes with the same diameter, a predetermined number of grinding balls are placed in the drum, the outer cylinder is sleeved on the outer wall of the drum, and the outer cylinder and the first end of the drum are sealed by a first bearing connected, the second end is provided with a window for taking out parts, and the window is sealed with the charging door; it also includes a driving mechanism arranged at the bottom of the base body, the driving mechanism is connected with the first bearing, and passes through driving the first bearing to rotate to drive the drum to rotate;
其中,所述滚筒壁上均匀设置有多个相同孔径的小孔,所述小孔的孔径小于所述磨球的直径。Wherein, a plurality of small holes of the same diameter are uniformly arranged on the wall of the drum, and the diameter of the small holes is smaller than the diameter of the grinding ball.
其中,还包括支撑结构,所述支撑结构包括第二轴承、第一支撑架和第二支撑架,所述第二轴承与所述第一轴承同轴,所述第一支撑架和所述第二支撑架固定在所述机体上,所述第一支撑架与所述外筒连接,用于支撑所述外筒的一端,所述第二支撑架与所述外筒连接,用于支撑所述外筒的另一端。Wherein, it also includes a support structure, the support structure includes a second bearing, a first support frame and a second support frame, the second bearing is coaxial with the first bearing, the first support frame and the first support frame Two supporting frames are fixed on the body, the first supporting frame is connected with the outer tube for supporting one end of the outer tube, the second supporting frame is connected with the outer tube for supporting the The other end of the outer cylinder.
其中,还包括超声波振动装置,所述超声波振动装置包括超声波换能器和超声波发生器,所述的超声波换能器安装在所述外筒上,所述超声波发生器固定所述机体上。Wherein, an ultrasonic vibration device is also included, and the ultrasonic vibration device includes an ultrasonic transducer and an ultrasonic generator, the ultrasonic transducer is installed on the outer cylinder, and the ultrasonic generator is fixed on the body.
其中,所述驱动机构包括电机和带轮,所述电机通过带动与所述第一轴承同轴的带轮带动所述滚筒转动。Wherein, the driving mechanism includes a motor and a pulley, and the motor drives the pulley coaxial with the first bearing to drive the drum to rotate.
其中,所述磨球为铬合金铸球、贝氏体磨球、马氏体复合组织球、铁磨球或高碳低合金磨球。Wherein, the grinding ball is a chromium alloy casting ball, a bainite grinding ball, a martensitic composite structure ball, an iron grinding ball or a high-carbon low-alloy grinding ball.
其中,还包括研磨液循环加热模块,所述研磨液循环加热模块包括研磨液入口、研磨液出口、加热装置和压缩泵,所述研磨液入口与所述压缩泵和所述机体连接,用于为循环研磨液和将新鲜研磨液注入外筒中提供通道,所述研磨液循环加热模块还设置有与所述机体连接的管道,所述管道用于废除废弃的研磨液。Wherein, it also includes a grinding liquid circulation heating module, and the grinding liquid circulation heating module includes a grinding liquid inlet, a grinding liquid outlet, a heating device and a compression pump, and the grinding liquid inlet is connected with the compression pump and the body for Channels are provided for circulating the grinding liquid and injecting fresh grinding liquid into the outer cylinder, and the grinding liquid circulating heating module is also provided with a pipeline connected to the body, and the pipeline is used for discarding the waste grinding liquid.
其中,还包括设置在所述研磨液出口的过滤器,用于过滤研磨过程中产生的废渣。Wherein, a filter arranged at the outlet of the grinding liquid is also included for filtering waste residue generated during the grinding process.
其中,所述第二轴承为双列深沟球轴承。Wherein, the second bearing is a double row deep groove ball bearing.
本发明实施例所提供的涂镀层结合力的检验方法及检验装置,与现有技术相比,具有以下优点:Compared with the prior art, the inspection method and inspection device for coating adhesion provided by the embodiments of the present invention have the following advantages:
本发明实施例提供的一种涂镀层结合力的检验方法,包括:A method for testing the bonding strength of coatings provided in the embodiments of the present invention includes:
将待检的涂镀层零件放入放置有预定数量磨球的滚筒中;Put the coated parts to be inspected into the drum with a predetermined number of grinding balls;
将所述滚筒浸在预定体积、预定温度的研磨液中;immersing the drum in a predetermined volume and temperature of grinding liquid;
设置所述滚筒转速、研磨时间,并进行预定时间的研磨;Set the rotating speed and grinding time of the drum, and perform grinding for a predetermined time;
检查所述零件涂镀层是否存在起泡、脱落现象,其中,所述滚筒的侧壁设置有多个小孔,所述小孔的直径小于所述磨球的直径;Check whether there are bubbles and shedding phenomena in the coating of the part, wherein the side wall of the drum is provided with a plurality of small holes, and the diameter of the small holes is smaller than the diameter of the grinding ball;
若是,判定所述涂镀层不合格,若否,判定所述涂镀层合格。If yes, it is determined that the coating is unqualified; if not, it is determined that the coating is qualified.
除此之外,本发明实施例还提供了一种涂镀层结合力的检验装置,包括机体、操作面板和装料门,所述机体的内部设置有滚筒和外筒,所述滚筒壁上均匀设置多个相同孔径的小孔,所述滚筒内放置有预定数量磨球,所述外筒套接在所述滚筒的外壁上,所述外筒和所述滚筒的第一端通过第一轴承密封连接,第二端设置有用于放取零件的窗口,所述窗口与装料门密封连接;还包括设置在所述基体底部的驱动机构,所述驱动机构与所述第一轴承连接,并通过带动所述第一轴承转动带动所述滚筒转动;In addition, the embodiment of the present invention also provides an inspection device for coating bonding force, which includes a machine body, an operation panel and a charging door. A drum and an outer cylinder are arranged inside the body, and the wall of the drum is uniformly arranged A plurality of small holes with the same diameter, a predetermined number of grinding balls are placed in the drum, the outer cylinder is sleeved on the outer wall of the drum, and the outer cylinder and the first end of the drum are sealed by a first bearing connected, the second end is provided with a window for taking out parts, and the window is sealed with the charging door; it also includes a driving mechanism arranged at the bottom of the base body, the driving mechanism is connected with the first bearing, and passes through driving the first bearing to rotate to drive the drum to rotate;
其中,所述滚筒壁上均匀设置有多个相同孔径的小孔,所述小孔的孔径小于所述磨球的直径。Wherein, a plurality of small holes of the same diameter are uniformly arranged on the wall of the drum, and the diameter of the small holes is smaller than the diameter of the grinding ball.
所述涂镀层结合力的检验方法以及检验装置,通过将需要检测的零件放入滚筒中,而滚筒内放置有预定数量的磨球,滚筒内通过侧壁的小孔与外筒内连通,使得外筒的研磨液进入滚筒,选择合适的转速、研磨液以及磨球,通过零件与滚筒壁、磨珠子的碰撞和摩擦,当外界作用力大于涂镀层与基本材料的结合力时,涂镀层脱离基体材料,零件涂镀层则有起泡、脱落现象,评判零件涂镀层结合力较差;当外界作用力小于涂镀层与基体材料的结合力时,涂镀层保留在基体材料上,评判零件涂镀层结合力较好原理简单、操作方便,与已有的热震法、划格法、胶粘法相比,能够实现快捷有效且百分之百的零件检验,还可根据待检零件材质选择不同的磨球和研磨液,设置研磨参数提供多种工作模式,实现不同零件涂镀层结合力的最优检验。The inspection method and the inspection device for the bonding force of the coating and plating layer are to put the parts to be inspected into the drum, and a predetermined number of grinding balls are placed in the drum, and the inside of the drum communicates with the inside of the outer cylinder through a small hole in the side wall, so that The grinding liquid of the outer cylinder enters the drum, select the appropriate speed, grinding liquid and grinding balls, through the collision and friction of the parts, the wall of the drum, and the grinding beads, when the external force is greater than the bonding force between the coating and the basic material, the coating will be detached The base material and the coating of the part have blistering and peeling phenomena, and the coating of the part is judged to have poor bonding force; when the external force is less than the bonding force between the coating and the base material, the coating remains on the base material, and the coating of the part is judged Good binding force The principle is simple and the operation is convenient. Compared with the existing thermal shock method, cross-cut method, and glue method, it can realize fast, effective and 100% part inspection. Different grinding balls and materials can be selected according to the material of the parts to be inspected. Grinding liquid, setting grinding parameters provides a variety of working modes to achieve the optimal inspection of the bonding force of coatings on different parts.
附图说明Description of drawings
为了更清楚地说明本发明实施例或现有技术中的技术方案,下面将对实施例或现有技术描述中所需要使用的附图作简单地介绍,显而易见地,下面描述中的附图是本发明的一些实施例,对于本领域普通技术人员来讲,在不付出创造性劳动的前提下,还可以根据这些附图获得其他的附图。In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings that need to be used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the accompanying drawings in the following description are For some embodiments of the present invention, those skilled in the art can also obtain other drawings based on these drawings without any creative work.
图1为本发明实施例提供的涂镀层结合力的检验方法的一种具体实施方式的步骤流程示意图;Fig. 1 is a schematic flow chart of the steps of a specific embodiment of the method for testing the adhesion of the coating layer provided by the embodiment of the present invention;
图2为本发明实施例提供的涂镀层结合力的检验装置的一种具体实施方式的结构示意图。Fig. 2 is a schematic structural view of a specific embodiment of a testing device for coating bonding force provided by an embodiment of the present invention.
具体实施方式detailed description
正如背景技术部分所述,现有技术不能实现快捷有效且百分之百的零件检验。As mentioned in the background art section, the existing technology cannot realize fast, effective and 100% parts inspection.
基于此,本发明实施例所提供了本发明实施例提供的一种涂镀层结合力的检验方法,包括:Based on this, the embodiment of the present invention provides a method for testing the adhesion of the coating and plating provided by the embodiment of the present invention, including:
将待检的涂镀层零件放入放置有预定数量磨球的滚筒中;Put the coated parts to be inspected into the drum with a predetermined number of grinding balls;
将所述滚筒浸在预定体积、预定温度的研磨液中;immersing the drum in a predetermined volume and temperature of grinding liquid;
设置所述滚筒转速、研磨时间,并进行预定时间的研磨;Set the rotating speed and grinding time of the drum, and perform grinding for a predetermined time;
检查所述零件涂镀层是否存在起泡、脱落现象,其中,所述滚筒的侧壁设置有多个小孔,所述小孔的直径小于所述磨球的直径;Check whether there are bubbles and shedding phenomena in the coating of the part, wherein the side wall of the drum is provided with a plurality of small holes, and the diameter of the small holes is smaller than the diameter of the grinding ball;
若是,判定所述涂镀层不合格,若否,判定所述涂镀层合格。If yes, it is determined that the coating is unqualified; if not, it is determined that the coating is qualified.
除此之外,本发明实施例还提供了一种涂镀层结合力的检验装置,包括机体、操作面板和装料门,所述机体的内部设置有滚筒和外筒,所述滚筒壁上均匀设置多个相同孔径的小孔,所述滚筒内放置有预定数量磨球,所述外筒套接在所述滚筒的外壁上,所述外筒和所述滚筒的第一端通过第一轴承密封连接,第二端设置有用于放取零件的窗口,所述窗口与装料门密封连接;还包括设置在所述基体底部的驱动机构,所述驱动机构与所述第一轴承连接,并通过带动所述第一轴承转动带动所述滚筒转动;In addition, the embodiment of the present invention also provides an inspection device for coating bonding force, which includes a machine body, an operation panel and a charging door. A drum and an outer cylinder are arranged inside the body, and the wall of the drum is uniformly arranged A plurality of small holes with the same diameter, a predetermined number of grinding balls are placed in the drum, the outer cylinder is sleeved on the outer wall of the drum, and the outer cylinder and the first end of the drum are sealed by a first bearing connected, the second end is provided with a window for taking out parts, and the window is sealed with the charging door; it also includes a driving mechanism arranged at the bottom of the base body, the driving mechanism is connected with the first bearing, and passes through driving the first bearing to rotate to drive the drum to rotate;
其中,所述滚筒壁上均匀设置有多个相同孔径的小孔,所述小孔的孔径小于所述磨球的直径。Wherein, a plurality of small holes of the same diameter are uniformly arranged on the wall of the drum, and the diameter of the small holes is smaller than the diameter of the grinding ball.
综上所述,本发明实施例提供的涂镀层结合力的检验方法以及检验装置,通过将需要检测的零件放入滚筒中,而滚筒内放置有预订数量的磨球,滚筒内通过侧壁的小孔与外筒内连通,使得外筒的研磨液进入滚筒,选择合适的转速、研磨液以及磨球,通过零件与滚筒壁、磨珠子的碰撞和摩擦,当外界作用力大于图镀层与基本材料的结合力时,涂镀层脱离基体材料,零件涂镀层则有起泡、脱落现象,评判零件涂镀层结合力较差;当外界作用力小于涂镀层与基体材料的结合力时,涂镀层保留在基体材料上,评判零件涂镀层结合力较好原理简单、操作方便,与已有的热震法、划格法、胶粘法相比,能够实现快捷有效且百分之百的零件检验,还可根据待检零件材质选择不同的磨球和研磨液,设置研磨参数提供多种工作模式,实现不同零件涂镀层结合力的最优检验。To sum up, in the inspection method and inspection device for coating bonding force provided by the embodiment of the present invention, the parts to be inspected are put into the drum, and a predetermined number of grinding balls are placed in the drum, and the grinding balls of the side wall pass through the drum. The small hole is connected with the inside of the outer cylinder, so that the grinding liquid of the outer cylinder enters the drum. Select the appropriate speed, grinding liquid and grinding balls. Through the collision and friction between the parts and the drum wall and grinding beads, when the external force is greater than that of the coating and the basic When the bonding force of the material is high, the coating layer is separated from the base material, and the coating layer of the part has blistering and falling off, and the bonding force of the coating layer of the part is judged to be poor; when the external force is less than the bonding force between the coating layer and the base material, the coating layer remains On the base material, the principle of judging the good bonding force of the coating and plating of the parts is simple and easy to operate. Compared with the existing thermal shock method, cross-cut method, and adhesive method, it can realize fast, effective and 100% part inspection. Different grinding balls and grinding liquids are selected for the material of the inspection parts, and the grinding parameters are set to provide a variety of working modes to achieve the optimal inspection of the coating bonding force of different parts.
为使本发明的上述目的、特征和优点能够更为明显易懂,下面结合附图对本发明的具体实施方式做详细的说明。In order to make the above objects, features and advantages of the present invention more comprehensible, specific implementations of the present invention will be described in detail below in conjunction with the accompanying drawings.
在以下描述中阐述了具体细节以便于充分理解本发明。但是本发明能够以多种不同于在此描述的其它方式来实施,本领域技术人员可以在不违背本发明内涵的情况下做类似推广。因此本发明不受下面公开的具体实施的限制。In the following description, specific details are set forth in order to provide a thorough understanding of the present invention. However, the present invention can be implemented in many other ways than those described here, and those skilled in the art can make similar extensions without departing from the connotation of the present invention. Accordingly, the invention is not limited to the specific implementations disclosed below.
请参考图1,图1为本发明实施例提供的涂镀层结合力的检验方法的一种具体实施方式的步骤流程示意图。Please refer to FIG. 1 . FIG. 1 is a schematic flow chart of the steps of a specific implementation of the method for testing the adhesion of coatings and plating provided by the embodiment of the present invention.
在一种具体实施方式中,所述涂镀层结合力的检验方法,包括:In a specific embodiment, the inspection method of the bonding force of the coating and plating includes:
步骤1,将待检的涂镀层零件放入放置有预定数量磨球的滚筒中;Step 1, put the coated parts to be inspected into a drum with a predetermined number of grinding balls;
步骤2,将所述滚筒浸在预定体积、预定温度的研磨液中;Step 2, immersing the roller in a grinding liquid of a predetermined volume and a predetermined temperature;
步骤3,设置所述滚筒转速、研磨时间,并进行预定时间的研磨;Step 3, setting the rotating speed and grinding time of the drum, and performing grinding for a predetermined time;
步骤4,检查零件涂镀层是否存在起泡、脱落现象,滚筒的侧壁设置有多个小孔,小孔的直径小于磨球的直径;Step 4, check whether there is foaming or peeling off of the coating layer of the part. There are many small holes on the side wall of the drum, and the diameter of the small holes is smaller than the diameter of the grinding ball;
若是,步骤5,判定涂镀层不合格,若否,步骤6,判定涂镀层合格。If yes, step 5, determine that the coating is unqualified, if not, step 6, determine that the coating is qualified.
需要说明的是,本发明中对滚筒的转速、研磨时间的设定可以在步骤1或步骤2之前,但是步骤2必须在步骤1之后,因为在研磨液的温度升高之后,再放入涂镀层零件存在安全隐患。It should be noted that in the present invention, the setting of the rotating speed and grinding time of the drum can be done before step 1 or step 2, but step 2 must be after step 1, because after the temperature of the grinding liquid is raised, the coating Plated parts present a safety hazard.
所述涂镀层结合力的检验方法,通过将需要检测的零件放入滚筒中,而滚筒内放置有预订数量的磨球,滚筒内通过侧壁的小孔与外筒内连通,使得外筒的研磨液进入滚筒,选择合适的转速、研磨液以及磨球,通过零件与滚筒壁、磨珠子的碰撞和摩擦,当外界作用力大于图镀层与基本材料的结合力时,涂镀层脱离基体材料,零件涂镀层则有起泡、脱落现象,评判零件涂镀层结合力较差;当外界作用力小于涂镀层与基体材料的结合力时,涂镀层保留在基体材料上,评判零件涂镀层结合力较好原理简单、操作方便,与已有的热震法、划格法、胶粘法相比,能够实现快捷有效且百分之百的零件检验,还可根据待检零件材质选择不同的磨球和研磨液,设置研磨参数提供多种工作模式,实现不同零件涂镀层结合力的最优检验。The test method for the bonding force of the coating layer is to put the parts to be detected into the drum, and a predetermined number of grinding balls are placed in the drum, and the inside of the drum is connected with the inside of the outer cylinder through the small hole in the side wall, so that the outer cylinder When the grinding liquid enters the drum, select the appropriate speed, grinding liquid and grinding balls, and through the collision and friction between the parts and the drum wall and grinding beads, when the external force is greater than the bonding force between the coating and the basic material, the coating will separate from the base material, The coating layer of the part has blistering and falling off, and the bonding force of the coating layer of the part is judged to be poor. The good principle is simple and easy to operate. Compared with the existing thermal shock method, scratch method and glue method, it can realize fast, effective and 100% parts inspection. Different grinding balls and grinding fluids can be selected according to the material of the parts to be inspected. Setting the grinding parameters provides a variety of working modes to achieve the optimal inspection of the bonding force of coatings on different parts.
为进一步提高检验效率,一般使用增加超声波扫描的方式,即在零件发生碰撞、摩擦的过程中,通过超声波扫描,能够快速达到临界值,降低研磨时间,因此,所述步骤3,设置所述滚筒转速、研磨时间,并进行预定时间的研磨,还包括:In order to further improve the inspection efficiency, the method of increasing ultrasonic scanning is generally used, that is, in the process of collision and friction of parts, through ultrasonic scanning, the critical value can be quickly reached and the grinding time can be reduced. Therefore, in the step 3, set the roller Rotational speed, grinding time, and grinding for a predetermined time, also includes:
对所述涂镀层零件进行超声波扫描。An ultrasonic scan is performed on the coated part.
需要说明的是,本发明对超声波的扫描的起始时间和停止时间以及扫描功率不做具体限定,一般是在研磨的过程中进行扫描。It should be noted that the present invention does not specifically limit the start time, stop time and scan power of ultrasonic scanning, and generally scans are performed during grinding.
在本发明中,也可以直接使用超声波对零件进行扫描,但是这种方式需要的时间较长,效果不是很明显,因此一般选用研磨和超声波扫描结合的方式,这里的超声波扫描类似超声波清洗。In the present invention, it is also possible to directly use ultrasonic waves to scan parts, but this method takes a long time and the effect is not very obvious. Therefore, the combination of grinding and ultrasonic scanning is generally used. The ultrasonic scanning here is similar to ultrasonic cleaning.
除此之外,本发明实施例还提供了一种涂镀层结合力的检验装置,如图2所示,包括机体1、操作面板11和装料门21,所述机体1的内部设置有滚筒22和外筒23,所述滚筒22壁上均匀设置多个相同孔径的小孔,所述滚筒22内放置有预定数量磨球,所述外筒23套接在所述滚筒22的外壁上,所述外筒23和所述滚筒22的第一端通过第一轴承24密封连接,第二端设置有用于放取零件的窗口,所述窗口与装料门21密封连接;还包括设置在所述基体底部的驱动机构,所述驱动机构与所述第一轴承24连接,并通过带动所述第一轴承24转动带动所述滚筒22转动;In addition, the embodiment of the present invention also provides an inspection device for coating adhesion, as shown in FIG. and an outer cylinder 23, a plurality of small holes of the same aperture are uniformly arranged on the wall of the cylinder 22, a predetermined number of grinding balls are placed in the cylinder 22, and the outer cylinder 23 is sleeved on the outer wall of the cylinder 22, so The first end of the outer cylinder 23 and the drum 22 is sealed and connected through the first bearing 24, and the second end is provided with a window for placing and taking parts, and the window is sealed and connected with the charging door 21; A driving mechanism at the bottom of the base body, the driving mechanism is connected to the first bearing 24, and drives the roller 22 to rotate by driving the first bearing 24 to rotate;
其中,所述滚筒22壁上均匀设置有多个相同孔径的小孔,所述小孔的孔径小于所述磨球的直径。Wherein, the wall of the drum 22 is uniformly provided with a plurality of small holes with the same diameter, and the diameter of the small holes is smaller than the diameter of the grinding balls.
本发明中的滚筒22和外筒23一般选用不锈钢材质制作。The drum 22 and the outer cylinder 23 in the present invention are generally made of stainless steel.
本发明对滚筒22壁上的小孔的孔径、数量以及排列方式不做具体限定。需要说明的是,本发明装置可根据待检零件材质选择不同种类、不同尺寸的磨球以及不同的研磨液,具体地,磨球可选择铬合金铸球,贝氏体或贝氏体、马氏体复合组织球铁磨球,高碳低合金磨球;研磨液可选择蒸馏水、硅油或者变压器油。The present invention does not specifically limit the diameter, quantity and arrangement of the small holes on the wall of the drum 22 . It should be noted that the device of the present invention can select different types and sizes of grinding balls and different grinding liquids according to the material of the parts to be inspected. Specifically, the grinding balls can be selected from chromium alloy cast balls, bainite or bainite, Tensile composite structure ductile iron grinding balls, high-carbon low-alloy grinding balls; grinding fluid can choose distilled water, silicone oil or transformer oil.
当然,本发明中可根据设置研磨参数提供多种工作模式,通过选择是否加入磨球和研磨液,以及选择是否使用加热装置43和超声波振动装置。Of course, the present invention can provide multiple working modes according to setting grinding parameters, by choosing whether to add grinding balls and grinding liquid, and whether to use heating device 43 and ultrasonic vibration device.
由于滚筒22是设置在机体1上的,外部还套接有外筒23,之间还有研磨液。由于滚筒22在转动的过程中,会造成较大的震动,与机体1的连接容易遭到破坏,影响该装置的正常运转,因此一般会对滚筒22以及外筒23与机体1的连接进行加固或固定,因此,所述涂镀层结合力的检验装置还包括支撑结构,所述支撑结构包括第二轴承61、第一支撑架62和第二支撑架63,所述第二轴承61与所述第一轴承24同轴,所述第一支撑架62和所述第二支撑架63固定在所述机体1上,所述第一支撑架62与所述外筒23连接,用于支撑所述外筒的一端,所述第二支撑架与所述外筒连接,用于支撑所述外筒的另一端。Since the drum 22 is arranged on the machine body 1, an outer cylinder 23 is sheathed on the outside, and there is a grinding liquid therebetween. Because the drum 22 will cause a large vibration during the rotation process, the connection with the body 1 is easily damaged, affecting the normal operation of the device, so the connection between the drum 22 and the outer cylinder 23 and the body 1 is generally reinforced Or fixed, therefore, the inspection device of described coating bonding strength also comprises support structure, and described support structure comprises second bearing 61, first support frame 62 and second support frame 63, and described second bearing 61 and described The first bearing 24 is coaxial, the first support frame 62 and the second support frame 63 are fixed on the body 1, and the first support frame 62 is connected with the outer cylinder 23 for supporting the At one end of the outer cylinder, the second support frame is connected to the outer cylinder for supporting the other end of the outer cylinder.
需要说明的是,本发明对第一支撑架62和第二支撑架63的材质以及尺寸和设置方式不做具体限定。It should be noted that the present invention does not specifically limit the material, size and arrangement of the first support frame 62 and the second support frame 63 .
为进一步提高检验的效率,一般还会通过增加对零件进行超声波扫描,在研磨的过程中,进一步增加零件的涂镀层和基体之间的震动,增大外界施加在涂镀层和机体之间的作用力,这样能够更加快速的达到涂镀层与基体的临界结合力,这里的临界结合力是指合格时的临界结合力。为此,所述涂镀层结合力的检验装置还包括超声波振动装置,所述超声波振动装置包括超声波换能器51和超声波发生器52,所述的超声波换能器51安装在所述外筒23上,所述超声波发生器52固定所述机体1上。需要说明的是,本发明对超声波换能器51和超声波发生器52不做具体限定。In order to further improve the efficiency of the inspection, it is generally necessary to increase the ultrasonic scanning of the parts. During the grinding process, the vibration between the coating and the substrate of the parts will be further increased, and the external force between the coating and the body will be increased. In this way, the critical bonding force between the coating and the substrate can be reached more quickly, and the critical bonding force here refers to the critical bonding force when it is qualified. For this reason, the inspection device of the bonding force of the coating layer also includes an ultrasonic vibration device, and the ultrasonic vibration device includes an ultrasonic transducer 51 and an ultrasonic generator 52, and the ultrasonic transducer 51 is installed on the outer cylinder 23 Above, the ultrasonic generator 52 is fixed on the body 1 . It should be noted that the present invention does not specifically limit the ultrasonic transducer 51 and the ultrasonic generator 52 .
需要说明的是,本发明对所述临界结合力的标准不做具体限定,因为对于不同的涂镀零件,临界结合力不同,但是对同一种零件,也可以依照所述涂镀层结合力的检验装置以及检验方法,测试出合格的零件,并将该过程中的设定的测试参数作为标准,如将测量过程中的磨球的种类、尺寸和数量,研磨液的种类、温度、体积,超声波扫描的功率、时间以及超声波扫描的起止时间等,如果在标准内检测的零件的涂镀层与基体在检测完之后正常,说明该零件的涂镀层结合力合格,否则,不合格。It should be noted that the present invention does not specifically limit the standard of the critical bonding force, because the critical bonding force is different for different coated parts, but for the same part, it can also be tested according to the coating bonding force. Device and inspection method to test qualified parts, and use the set test parameters in the process as standards, such as the type, size and quantity of grinding balls in the measurement process, the type, temperature, volume of grinding liquid, ultrasonic Scanning power, time, start and end time of ultrasonic scanning, etc., if the coating and substrate of the parts detected within the standard are normal after the inspection, it means that the coating bonding force of the part is qualified, otherwise, it is unqualified.
驱动机构的作用是带动滚筒22进行转动,驱动机构一般安装在滚筒22的正下方,但是这样会大大增加检验装置的高度,故而,一般所述驱动机构包括电机31和带轮32,所述电机31通过带动与所述第一轴承24同轴的带轮32带动所述滚筒22转动。The function of the driving mechanism is to drive the drum 22 to rotate. The driving mechanism is generally installed directly below the drum 22, but this will greatly increase the height of the inspection device. Therefore, generally the driving mechanism includes a motor 31 and a pulley 32. The motor 31 drives the pulley 32 coaxial with the first bearing 24 to drive the drum 22 to rotate.
所述磨球一般为铬合金铸球、贝氏体磨球、马氏体复合组织球、铁磨球或高碳低合金磨球,或者其它材质的磨球,根据涂镀零件的材质选择合适的磨球。The grinding balls are generally chromium alloy casting balls, bainite grinding balls, martensitic composite structure balls, iron grinding balls or high-carbon low-alloy grinding balls, or grinding balls of other materials. grinding balls.
由于零件可能的工作温度范围较高或者较低,并不是在室温下进行工作,这样直接在室温下检测出的零件的涂镀层与基体的结合力,与实际工作环境中的涂镀层与基体的结合力差别较大。Since the parts may work in a higher or lower temperature range, they do not work at room temperature, so the bonding force between the coating and the substrate of the part detected directly at room temperature is different from the coating and the substrate in the actual working environment. The bonding strength varies greatly.
为避免这一情况的发生,在检验高温环境下的结合力时,可以在模拟高温环境下零件的涂镀层与基体的结合力,对研磨液进行加热,即所述涂镀层结合力的检验装置还包括研磨液循环加热模块,所述研磨液循环加热模块包括研磨液入口41、研磨液出口42、加热装置43和压缩泵44,所述研磨液入口41与所述压缩泵44和所述机体1连接,用于为循环研磨液和将新鲜研磨液注入外筒23中提供通道,所述研磨液循环加热模块还设置有与所述机体连接的管道,所述管道用于废除废弃的研磨液,所述管道用于废除废弃的研磨液。In order to avoid this situation, when testing the bonding force in a high temperature environment, the bonding force between the coating and the substrate of the part under the high temperature environment can be simulated, and the grinding liquid can be heated, which is the testing device for the bonding force of the coating. Also includes a grinding liquid circulation heating module, the grinding liquid circulation heating module includes a grinding liquid inlet 41, a grinding liquid outlet 42, a heating device 43 and a compression pump 44, and the grinding liquid inlet 41 is connected to the compression pump 44 and the body 1 connection, used to provide passages for circulating the grinding liquid and injecting fresh grinding liquid into the outer cylinder 23, the grinding liquid circulation heating module is also provided with a pipeline connected to the body, and the pipeline is used to abolish the waste grinding liquid , the pipeline is used to abolish the waste grinding liquid.
相应的如果需要进行在低温环境检验零件的涂镀层与基体的结合力时,将加热装置43更换为制冷装置即可。Correspondingly, if it is necessary to test the bonding force between the coating layer of the part and the substrate in a low-temperature environment, the heating device 43 can be replaced with a cooling device.
当然,为了更加准确的记录实施的温度,可以通过使用温度计测量研磨液的温度,来获得实际的零件所处的温度。Of course, in order to record the actual temperature more accurately, the temperature of the actual part can be obtained by measuring the temperature of the grinding liquid with a thermometer.
由于研磨液在使用后,可能存在在检验过程中,涂镀层发生脱离的现象,污染研磨液,形成废渣影响正常的使用,一般在在所述研磨液出口41设置过滤器,用于过滤研磨过程中产生的废渣,这样研磨液就可以循环使用,降低成本。本发明对所述过滤器的结构以及安装方式不做具体限定。由于第一轴承24是带动滚筒22转动的,第二轴承61是起到支撑的作用,就需要有较高的结构强度,第二轴承61一般选用双列深沟球轴承。Since the grinding fluid may be detached during the inspection process after use, polluting the grinding fluid and forming waste residues that affect normal use, a filter is generally installed at the grinding fluid outlet 41 to filter the grinding process The waste slag generated in the process can be recycled so that the grinding liquid can be recycled and the cost can be reduced. The present invention does not specifically limit the structure and installation method of the filter. Since the first bearing 24 drives the drum 22 to rotate, and the second bearing 61 plays a supporting role, it needs to have higher structural strength. The second bearing 61 generally selects double-row deep groove ball bearings.
需要说明的是,在本发明中,滚筒22的转动的轴线方向不一定必须是竖直方向,有时为增加在同等转速下零件受到的加速度,一般将滚筒22横向设置,这样涂镀层结合力的检验装置的高度就可以较低,便于搬运,便于从上部加入研磨液,对放置房间的要求较低。It should be noted that, in the present invention, the axis direction of the rotation of the drum 22 does not necessarily have to be the vertical direction. Sometimes, in order to increase the acceleration that the parts are subjected to at the same rotational speed, the drum 22 is generally arranged laterally, so that the bonding force of the coating layer can be improved. The height of the inspection device can be lower, which is convenient for handling and adding grinding liquid from the upper part, and has lower requirements for the room where it is placed.
综上所述,本发明实施例提供的涂镀层结合力的检验方法以及检验装置,通过将需要检测的零件放入滚筒中,而滚筒内放置有预定数量的磨球,滚筒内通过侧壁的小孔与外筒内连通,使得外筒的研磨液进入滚筒,选择合适的转速、研磨液以及磨球,通过零件与滚筒壁、磨球的碰撞和摩擦,当外界作用力大于涂镀层与基本材料的结合力时,涂镀层脱离基体材料,零件涂镀层则有起泡、脱落现象,评判零件涂镀层结合力较差;当外界作用力小于涂镀层与基体材料的结合力时,涂镀层保留在基体材料上,评判零件涂镀层结合力较好原理简单、操作方便,与已有的热震法、划格法、胶粘法相比,能够实现快捷有效且百分之百的零件检验,还可根据待检零件材质选择不同的磨球和研磨液,设置研磨参数提供多种工作模式,实现不同零件涂镀层结合力的最优检验。To sum up, in the inspection method and inspection device for the bonding force of the coating provided by the embodiment of the present invention, the parts to be inspected are put into the drum, and a predetermined number of grinding balls are placed in the drum. The small hole communicates with the outer cylinder so that the grinding liquid in the outer cylinder enters the drum. Select the appropriate speed, grinding liquid and grinding balls. Through the collision and friction between the parts and the drum wall and grinding balls, when the external force is greater than that of the coating layer and the basic When the bonding force of the material is high, the coating layer is separated from the base material, and the coating layer of the part has blistering and falling off, and the bonding force of the coating layer of the part is judged to be poor; when the external force is less than the bonding force between the coating layer and the base material, the coating layer remains On the base material, the principle of judging the good bonding force of the coating and plating of the parts is simple and easy to operate. Compared with the existing thermal shock method, cross-cut method, and adhesive method, it can realize fast, effective and 100% part inspection. Different grinding balls and grinding liquids are selected for the material of the inspection parts, and the grinding parameters are set to provide a variety of working modes to achieve the optimal inspection of the coating bonding force of different parts.
以上对本发明所提供的涂镀层结合力的检验方法以及检验装置进行了详细介绍。本文中应用了具体个例对本发明的原理及实施方式进行了阐述,以上实施例的说明只是用于帮助理解本发明的方法及其核心思想。应当指出,对于本技术领域的普通技术人员来说,在不脱离本发明原理的前提下,还可以对本发明进行若干改进和修饰,这些改进和修饰也落入本发明权利要求的保护范围内。The inspection method and inspection device for the bonding force of the coating layer provided by the present invention have been introduced in detail above. In this paper, specific examples are used to illustrate the principle and implementation of the present invention, and the descriptions of the above embodiments are only used to help understand the method and core idea of the present invention. It should be pointed out that for those skilled in the art, without departing from the principle of the present invention, some improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.
Claims (10)