CN105385063A - PVC/PVF co-extrusion pipe and preparation method thereof - Google Patents

PVC/PVF co-extrusion pipe and preparation method thereof Download PDF

Info

Publication number
CN105385063A
CN105385063A CN201510908748.6A CN201510908748A CN105385063A CN 105385063 A CN105385063 A CN 105385063A CN 201510908748 A CN201510908748 A CN 201510908748A CN 105385063 A CN105385063 A CN 105385063A
Authority
CN
China
Prior art keywords
pvf
pvc
coextrusion
layer
temperature
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510908748.6A
Other languages
Chinese (zh)
Other versions
CN105385063B (en
Inventor
龙国才
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Suzhou Shengxin Management Industry Co ltd
Original Assignee
Heshan Suxie Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Heshan Suxie Technology Co Ltd filed Critical Heshan Suxie Technology Co Ltd
Priority to CN201510908748.6A priority Critical patent/CN105385063B/en
Publication of CN105385063A publication Critical patent/CN105385063A/en
Application granted granted Critical
Publication of CN105385063B publication Critical patent/CN105385063B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种PVC/PVF共挤出管材及其制备方法,通过在PVC管材配方中添加PVC高效改性剂SX630,并采用共挤出的方法在PVC管材的内层或外层添加了一层PVF树脂层,大大提高了PVC管材的抗冲击、耐压性、耐蠕变、抗老化等性能。A PVC/PVF co-extrusion pipe and its preparation method, by adding PVC high-efficiency modifier SX630 to the PVC pipe formula, and adding a layer of PVF resin to the inner or outer layer of the PVC pipe by co-extrusion Layer, greatly improving the impact resistance, pressure resistance, creep resistance, aging resistance and other properties of PVC pipes.

Description

一种PVC/PVF共挤出管材及其制备方法A kind of PVC/PVF coextrusion pipe material and preparation method thereof

技术领域technical field

本发明属于塑料管材制造领域,尤其涉及一种PVC/PVF共挤出管材及其制备方法。The invention belongs to the field of plastic pipe manufacture, and in particular relates to a PVC/PVF co-extruded pipe and a preparation method thereof.

背景技术Background technique

聚氯乙烯(PVC)管材是目前国内外产量最大、使用最广泛的塑料管材之一,广泛用于建筑给水、排水,埋地给水、排水,电工管套,农业和工业用管等领域。PVC-U管材具有高规模、高强度且价格较低等优点,是PVC管材市场领域中应用最广泛的品种之一,但由于PVC-U管材的脆性较大,在运输、安装、施工等过程中容易破裂。抗冲改性聚氯乙烯管材(即PVC-M管材)除了具有PVC-U管材的特点外,抗冲击性能显著提高,极大地降低了脆性开裂的可能性。Polyvinyl chloride (PVC) pipe is currently one of the largest and most widely used plastic pipes at home and abroad. It is widely used in building water supply and drainage, buried water supply and drainage, electrical pipe sleeves, agricultural and industrial pipes and other fields. PVC-U pipe has the advantages of high scale, high strength and low price. It is one of the most widely used varieties in the PVC pipe market. easy to break. In addition to the characteristics of PVC-U pipes, impact-modified polyvinyl chloride pipes (namely, PVC-M pipes) have significantly improved impact resistance, which greatly reduces the possibility of brittle cracking.

然而,目前市场上已经出现的PVC管材,由于配方、原料及加工工艺不够合理,管材的耐候性及耐蠕变性并不理想。However, due to the unreasonable formula, raw materials and processing technology of the PVC pipes that have appeared on the market, the weather resistance and creep resistance of the pipes are not ideal.

发明内容Contents of the invention

本发明的目的在于针对现有技术的不足,提供一种PVC/PVF共挤出管材及其制备方法,提高了PVC管材的耐候性、耐压性、抗冲性等。The purpose of the present invention is to provide a PVC/PVF co-extrusion pipe and its preparation method to improve the weather resistance, pressure resistance and impact resistance of the PVC pipe.

为实现上述目的,本发明采用如下技术方案:To achieve the above object, the present invention adopts the following technical solutions:

一种制备PVC/PVF共挤出管材的方法,其特征在于包括以下步骤:A method for preparing PVC/PVF co-extrusion pipes is characterized in that comprising the following steps:

(1)将制作PVC的原料放入高低速混合机中搅拌混合均匀,转速为1000-2000RPM,混合时间为10-20分钟;混合至温度110-120℃时将物料放到低速混合机中,转速为400-500RPM,待混合至温度40-50℃出料得混合物料;(1) Put the raw materials for making PVC into a high-low speed mixer and mix them evenly, the speed is 1000-2000RPM, and the mixing time is 10-20 minutes; when the temperature is 110-120°C, put the materials into the low-speed mixer, The rotation speed is 400-500RPM, and the mixed material is obtained after being mixed until the temperature is 40-50°C;

(2)双层共挤:将步骤(1)所得混合物料与PVF树脂分别投入双螺杆单机共挤出机或双螺杆双机共挤出机料斗内,加热挤出后,通过双层复合模具成型并输出,喂料转速10-40RPM,主机转速30-150RPM,机筒温度150-200℃,机头温度为150-205℃;(2) Double-layer co-extrusion: put the mixed material and PVF resin obtained in step (1) into the hopper of a twin-screw single-machine co-extruder or a twin-screw double-machine co-extruder, and after heating and extruding, pass through a double-layer composite mold Forming and output, feeding speed 10-40RPM, host speed 30-150RPM, barrel temperature 150-200℃, head temperature 150-205℃;

(3)冷却、牵引、切割,得到PVC/PVF共挤出管材。(3) Cooling, pulling, and cutting to obtain PVC/PVF co-extruded pipes.

优选的,冷却为真空定型冷却,步骤如下:采用真空喷射水雾来瞬间降温,水温分三段,第一段水温在60-80℃并喷射2-5min,第二段水温在10-30℃并喷射5-10min,第三段水温在5-8℃并喷射5-10min,水可以循环回用,真空度保持在-0.02-0.06MPa。Preferably, the cooling is vacuum setting cooling, and the steps are as follows: use vacuum spray water mist to instantly cool down, the water temperature is divided into three stages, the first stage water temperature is 60-80°C and spray for 2-5min, the second stage water temperature is 10-30°C And spray for 5-10 minutes, the third stage water temperature is 5-8 ℃ and spray for 5-10 minutes, the water can be recycled, and the vacuum degree is kept at -0.02-0.06MPa.

本发明还提供一种PVC/PVF共挤出管材,其特征在于,由以下重量份的原料制成:The present invention also provides a PVC/PVF co-extrusion pipe, which is characterized in that it is made of the following raw materials in parts by weight:

优选的,所述的PVC树脂为SG-5型树脂。Preferably, the PVC resin is SG-5 type resin.

优选的,所述的稳定剂为铅盐稳定剂、锡盐稳定剂、钙锌稳定剂、稀土稳定剂。Preferably, the stabilizer is lead salt stabilizer, tin salt stabilizer, calcium zinc stabilizer, rare earth stabilizer.

优选的,所述的稳定剂为钙锌稳定剂。Preferably, the stabilizer is calcium zinc stabilizer.

优选的,所述的钛白粉为金红石型钛白粉或锐钛型钛白粉。Preferably, the titanium dioxide is rutile titanium dioxide or anatase titanium dioxide.

一种制备上述PVC/PVF共挤出管材的方法,其特征在于包括以下步骤:A method for preparing the above-mentioned PVC/PVF co-extrusion pipe, is characterized in that comprising the following steps:

(1)配料:按配比称量各种原料;(1) Ingredients: Weigh various raw materials according to the ratio;

(2)混料:将PVC树脂、轻钙、稳定剂、SX630、硬脂酸、石蜡和钛白粉放入高低速混合机中搅拌混合均匀,转速为1000-2000RPM,混合时间为10-20分钟,混合至温度110-120℃时将物料放到低速混合机中,转速400-500RPM,待混合至温度40-50℃出料得混合物料;(2) Mixing: Put PVC resin, light calcium, stabilizer, SX630, stearic acid, paraffin and titanium dioxide into a high-low speed mixer and mix evenly. The speed is 1000-2000RPM, and the mixing time is 10-20 minutes. When mixing to a temperature of 110-120°C, put the material into a low-speed mixer at a speed of 400-500RPM, and wait until the temperature is 40-50°C to discharge to obtain a mixed material;

(3)双层共挤:将混合物料与PVF树脂分别投入双螺杆单机或双螺杆双机料斗内,加热挤出后,通过双层共挤复合模具成型并输出,喂料转速10-40RPM,主机转速30-150RPM,机筒温度150-200℃,机头温度为150-205℃;(3) Double-layer co-extrusion: put the mixed material and PVF resin into the hopper of twin-screw single machine or twin-screw double-machine respectively, after heating and extruding, shape and output through double-layer co-extrusion composite mold, feeding speed 10-40RPM, The speed of the main engine is 30-150RPM, the temperature of the barrel is 150-200°C, and the temperature of the head is 150-205°C;

(4)冷却、牵引、切割,得到PVC/PVF共挤出管材。(4) Cooling, pulling, and cutting to obtain PVC/PVF co-extruded pipes.

优选的,上述冷却为真空定型冷却,步骤如下:采用真空喷射水雾来瞬间降温,水温分三段,第一段水温在60-80℃并喷射2-5min,第二段水温在10-30℃并喷射5-10min,第三段水温在5-8℃并喷射5-10min,水可以循环回用,真空度保持在-0.02-0.06MPa;Preferably, the above-mentioned cooling is vacuum setting cooling, and the steps are as follows: Use vacuum spray water mist to cool down instantly, the water temperature is divided into three sections, the first section is at 60-80°C and sprayed for 2-5min, the second section is at 10-30°C ℃ and spray for 5-10 minutes, the third stage water temperature is 5-8 ℃ and spray for 5-10 minutes, the water can be recycled, and the vacuum degree is kept at -0.02-0.06MPa;

优选的,所述的PVC/PVF共挤出管材的外层为PVC层,内层为PVF层;或外层为PVF层,内层为PVC层。Preferably, the outer layer of the PVC/PVF co-extruded pipe is a PVC layer, and the inner layer is a PVF layer; or the outer layer is a PVF layer, and the inner layer is a PVC layer.

优选的,PVF树脂层为10-20μm。Preferably, the PVF resin layer is 10-20 μm.

所述SX630是由鹤山塑协塑料加工技术研究所生产的PVC高效改性剂。The SX630 is a high-efficiency PVC modifier produced by the Plastic Processing Technology Research Institute of Heshan Plastic Association.

SX630是一种PVC高效改性剂,采用无机粒子改性PVC,无机粒子以纳米尺寸在有机聚合物基体中形成的有机/无机粒子间的相互作用而形成的核/壳与网状的共挤出结构,由于分散相的纳米尺寸效应、大的比表面积和强的界面结合,使共挤出材料具有优异的物理力学性能和特殊的功能,如:韧性好,强度高,耐蠕变,易加工以及抗紫外线等。将PVC的优良品性充分发挥,同时弥补了PVC的性能缺陷,从而达到增强增韧的目的。SX630 is a high-efficiency modifier for PVC. It uses inorganic particles to modify PVC. Inorganic particles are formed by the interaction between organic/inorganic particles in the organic polymer matrix in nanometer size. The co-extrusion of the core/shell and the network is formed. Due to the nano-size effect of the dispersed phase, large specific surface area and strong interfacial bonding, the co-extrusion material has excellent physical and mechanical properties and special functions, such as: good toughness, high strength, creep resistance, easy processing and UV resistance. Give full play to the excellent properties of PVC, and at the same time make up for the performance defects of PVC, so as to achieve the purpose of strengthening and toughening.

PVF树脂由氟和氟碳分子的共聚体挤压而成。为含氟或氟碳的共聚物,比任何聚合物具有更大的化学结合力和结构稳定性。PVF薄膜朝横向和纵向伸展,从而形成分子晶格,大大提高了它的物理性能。PVF薄膜对日照、化学溶剂、酸碱腐蚀、湿气和氧化作用的抵抗力和耐久性提高显著。挤压成型的PVF膜表面光滑细腻,全无滚涂或喷涂时表面产生的条纹、橘皮、微皱之类缺陷。采用PVC-PVF共挤出制成的PVC/PVF共挤出管材,PVF层与PVC层的界面能够很好的熔合和粘合,不会造成管材的分层和脱落。PVF resin is extruded from a copolymer of fluorine and fluorocarbon molecules. It is a copolymer containing fluorine or fluorocarbon, which has greater chemical bonding and structural stability than any polymer. The PVF film is stretched horizontally and vertically to form a molecular lattice, which greatly improves its physical properties. The resistance and durability of PVF film to sunlight, chemical solvents, acid and alkali corrosion, moisture and oxidation are significantly improved. The surface of the extruded PVF film is smooth and delicate, free of defects such as streaks, orange peel, and micro-wrinkles on the surface during roll coating or spraying. The PVC/PVF co-extrusion pipe made of PVC-PVF co-extrusion, the interface between the PVF layer and the PVC layer can be well fused and bonded without causing delamination and shedding of the pipe.

本发明中采用的共挤出技术为本领域常用的技术,如中国专利申请CN103388712A公开了一种复合管材,它是由外层抗老化层与内层耐热层通过单螺杆双层共挤出而成的,另外,中国专利申请CN201721024U公开了一种复合共挤锥形螺杆挤出机,实现了单机双层共挤出,减少共挤出机组主机数,节省了投资和设备占地面积。该两份文件以引用的方式结合到本文中。The co-extrusion technology adopted in the present invention is a commonly used technology in the art. For example, Chinese patent application CN103388712A discloses a composite pipe, which is co-extruded by a single-screw double-layer by an outer anti-aging layer and an inner heat-resistant layer. In addition, Chinese patent application CN201721024U discloses a compound co-extrusion conical screw extruder, which realizes single-machine double-layer co-extrusion, reduces the number of hosts of the co-extrusion unit, and saves investment and equipment footprint. Both documents are incorporated herein by reference.

本发明的有益效果是:本发明生产的PVC/PVF管材,通过在PVC管材配方中添加PVC高效改性剂SX630,并采用共挤出的方法在PVC管材的内层或外层添加了一层PVF树脂层,大大提高了管材的抗冲击、耐压性、耐蠕变、抗老化等性能。The beneficial effects of the present invention are: the PVC/PVF pipe produced by the present invention, by adding PVC high-efficiency modifier SX630 to the PVC pipe formula, and adopting the method of co-extrusion to add a layer to the inner or outer layer of the PVC pipe The PVF resin layer greatly improves the impact resistance, pressure resistance, creep resistance and aging resistance of the pipe.

具体实施方式detailed description

实施例1Example 1

一种PVC/PVF共挤出管材,由以下重量份的原料制成:A PVC/PVF co-extruded pipe made of the following raw materials in parts by weight:

SX630是由鹤山塑协塑料加工技术研究所生产的PVC高效改性剂。SX630 is a high-efficiency PVC modifier produced by the Plastic Processing Technology Research Institute of Heshan Plastic Association.

一种PVC/PVF共挤出管材的制备方法,包括以下步骤:A preparation method for PVC/PVF co-extruded pipes, comprising the following steps:

(1)配料:按配比称量各种原料(1) Ingredients: Weigh various raw materials according to the ratio

(2)混料:将SG-5型PVC树脂、轻钙、钙锌稳定剂、SX630、硬脂酸、石蜡和金红石型钛白粉放入高低速混合机中充分搅拌混合均匀,转速为1000RPM,混合时间为10分钟,混合至温度110℃时将物料放到低速混合机中,转速40RPM,待混合至温度40℃出料得混合物料;(2) Mixing: put SG-5 type PVC resin, light calcium, calcium zinc stabilizer, SX630, stearic acid, paraffin and rutile titanium dioxide into a high and low speed mixer and mix well, the speed is 1000RPM, The mixing time is 10 minutes. When the temperature is 110°C, put the material into a low-speed mixer at a speed of 40 RPM. After mixing until the temperature is 40°C, the mixed material is discharged;

(3)双层共挤:将混合物料与PVF树脂通过上料机卸入双螺杆单机共挤出机料斗内,加热挤出后,通过双层共挤复合模具成型并输出,混合物料为内层,PVF树脂为外层,PVF树脂层为10μm,喂料转速10RPM,主机转速30RPM,机筒温度150℃,机头温度为150℃;(3) Double-layer co-extrusion: The mixed material and PVF resin are discharged into the hopper of the twin-screw single-machine co-extruder through the feeder, and after heating and extruding, they are formed and output through the double-layer co-extruded composite mold. Layer, PVF resin is the outer layer, the PVF resin layer is 10μm, the feeding speed is 10RPM, the main engine speed is 30RPM, the barrel temperature is 150°C, and the head temperature is 150°C;

(4)真空定型冷却:采用真空喷射水雾来瞬间降温,水温分三段,第一段水温在60℃并喷射2min,第二段水温在10℃并喷射5min,第三段水温在5℃并喷射5min,水可以循环回用,真空度保持在-0.02MPa;(4) Vacuum shaping cooling: Use vacuum spray water mist to cool down instantly. The water temperature is divided into three sections. The first section has a water temperature of 60°C and sprays for 2 minutes, the second section has a water temperature of 10°C and sprays for 5 minutes, and the third section has a water temperature of 5°C. And spray for 5 minutes, the water can be recycled, and the vacuum degree is kept at -0.02MPa;

(5)牵引,切割,得到PVC/PVF共挤出管材。(5) Traction and cutting to obtain PVC/PVF co-extruded pipes.

实施例2Example 2

一种PVC/PVF共挤出管材,由以下重量份的原料制成:A PVC/PVF co-extruded pipe made of the following raw materials in parts by weight:

SX630是由鹤山塑协塑料加工技术研究所生产的PVC高效改性剂。SX630 is a high-efficiency PVC modifier produced by the Plastic Processing Technology Research Institute of Heshan Plastic Association.

一种PVC/PVF共挤出管材的制备方法,包括以下步骤:A preparation method for PVC/PVF co-extruded pipes, comprising the following steps:

(1)配料:按配比称量各种原料(1) Ingredients: Weigh various raw materials according to the ratio

(2)混料:将SG-5型PVC树脂、轻钙、钙锌稳定剂、SX630、硬脂酸、石蜡和金红石型钛白粉放入高低速混合机中充分搅拌混合均匀,转速为1500RPM,混合时间为15分钟,混合至温度115℃时将物料放到低速混合机中,转速450RPM,待混合至温度45℃出料得混合物料;(2) Mixing: Put SG-5 type PVC resin, light calcium, calcium zinc stabilizer, SX630, stearic acid, paraffin and rutile titanium dioxide into a high and low speed mixer and mix well, the speed is 1500RPM, The mixing time is 15 minutes. When the temperature is 115°C, put the material into a low-speed mixer with a rotation speed of 450 RPM. After mixing to a temperature of 45°C, the mixed material is discharged;

(3)双层共挤:将混合物料与PVF树脂通过上料机卸入双螺杆单机共挤出机料斗内,加热挤出后,通过双层共挤复合模具成型并输出,混合物料为内层,PVF树脂为外层,PVF树脂层为15μm,喂料转速25RPM,主机转速100RPM,机筒温度170℃,机头温度为175℃;(3) Double-layer co-extrusion: The mixed material and PVF resin are discharged into the hopper of the twin-screw single-machine co-extruder through the feeder, and after heating and extruding, they are formed and output through the double-layer co-extruded composite mold. Layer, PVF resin is the outer layer, the PVF resin layer is 15μm, the feeding speed is 25RPM, the host speed is 100RPM, the barrel temperature is 170°C, and the head temperature is 175°C;

(4)真空定型冷却:采用真空喷射水雾来瞬间降温,水温分三段,第一段水温在70℃并喷射3min,第二段水温在50℃并喷射7min,第三段水温在6℃并喷射7min,水可以循环回用,真空度保持在-0.015MPa;(4) Vacuum shaping cooling: Use vacuum spray water mist to cool down instantly. The water temperature is divided into three sections. The first section has a water temperature of 70°C and sprays for 3 minutes, the second section has a water temperature of 50°C and sprays for 7 minutes, and the third section has a water temperature of 6°C. And spray for 7 minutes, the water can be recycled, and the vacuum degree is kept at -0.015MPa;

(5)牵引,切割,得到PVC/PVF共挤出管材。(5) Traction and cutting to obtain PVC/PVF co-extruded pipes.

实施例3Example 3

一种PVC/PVF共挤出管材,由以下重量份的原料制成:A PVC/PVF co-extruded pipe made of the following raw materials in parts by weight:

SX630是由鹤山塑协塑料加工技术研究所生产的PVC高效改性剂。SX630 is a high-efficiency PVC modifier produced by the Plastic Processing Technology Research Institute of Heshan Plastic Association.

一种PVC/PVF共挤出管材的制备方法,包括以下步骤:A preparation method for PVC/PVF co-extruded pipes, comprising the following steps:

(1)配料:按配比称量各种原料(1) Ingredients: Weigh various raw materials according to the ratio

(2)混料:将SG-5型PVC树脂、轻钙、钙锌稳定剂、SX630、硬脂酸、石蜡和金红石型钛白粉放入高低速混合机中充分搅拌混合均匀,转速为2000RPM,混合时间为20分钟,混合至温度120℃时将物料放到低速混合机中,转速500RPM,待混合至温度50℃出料得混合物料;(2) Mixing: put SG-5 type PVC resin, light calcium, calcium zinc stabilizer, SX630, stearic acid, paraffin and rutile titanium dioxide into a high and low speed mixer and mix well, the speed is 2000RPM, The mixing time is 20 minutes. When the temperature is 120°C, put the material into a low-speed mixer with a rotation speed of 500 RPM. After mixing to a temperature of 50°C, the mixed material is discharged;

(3)双层共挤:将混合物料与PVF树脂通过上料机卸入双螺杆单机共挤出机料斗内,加热挤出后,通过双层共挤复合模具成型并输出,混合物料为内层,PVF树脂为外层,PVF树脂层为20μm,喂料转速40RPM,主机转速150RPM,机筒温度200℃,机头温度为205℃;(3) Double-layer co-extrusion: The mixed material and PVF resin are discharged into the hopper of the twin-screw single-machine co-extruder through the feeder, and after heating and extruding, they are formed and output through the double-layer co-extruded composite mold. Layer, PVF resin is the outer layer, the PVF resin layer is 20μm, the feeding speed is 40RPM, the host speed is 150RPM, the barrel temperature is 200°C, and the head temperature is 205°C;

(4)真空定型冷却:采用真空喷射水雾来瞬间降温,水温分三段,第一段水温在80℃并喷射5min,第二段水温在30℃并喷射10min,第三段水温在8℃并喷射10min,水可以循环回用,真空度保持在0.01MPa;(4) Vacuum shaping cooling: Use vacuum spray water mist to cool down instantly. The water temperature is divided into three stages. The first stage is at 80°C and sprayed for 5 minutes. The second stage is at 30°C and sprayed for 10 minutes. The third stage is at 8°C. And spray for 10 minutes, the water can be recycled, and the vacuum degree is kept at 0.01MPa;

(5)牵引,切割,得到PVC/PVF共挤出管材。(5) Traction and cutting to obtain PVC/PVF co-extruded pipes.

实施例4Example 4

本发明的各实施例PVC/PVF共挤出管材性能检测结果如下表所示:Each embodiment of the present invention PVC/PVF co-extruded pipe performance test results are shown in the following table:

从上表可以看出,与PVC-M管材相比,本发明所制得的PVC/PVF组合管材的拉伸强度、断裂生长率、抗击冲性能、耐候性都有所提高,且符合QB/T2480指标。As can be seen from the above table, compared with the PVC-M pipe, the tensile strength, fracture growth rate, impact resistance, and weather resistance of the PVC/PVF composite pipe prepared by the present invention are all improved, and meet QB/PVF T2480 indicators.

Claims (10)

1. prepare a method for PVC/PVF coextrusion tubing, it is characterized in that comprising the following steps:
(1) raw material making PVC is put into high low speed mixer to be uniformly mixed, rotating speed is 1000-2000RPM, and mixing time is 10-20 minute; Be put in low speed mixer by material when being mixed to temperature 110-120 DEG C, rotating speed is 400-500RPM, to be mixedly obtains mixture to discharging during temperature 40-50 DEG C;
(2) double-layer coextrusion: step (1) gained mixture and PVF resin are dropped into respectively in twin screw unit coextrusion machine or twin screw two-shipper coextrusion machine hopper, add hot-extrudable after, shaping and export by double-layer coextrusion composite die, feeding rotating speed 10-40RPM, 30-150RPM, barrel zone temperature 150-200 DEG C, head temperature is 150-205 DEG C;
(3) cool, draw, cut, obtain PVC/PVF coextrusion tubing.
2. a kind of method preparing PVC/PVF coextrusion tubing according to claim 1, it is characterized in that being cooled to Vacuum shaping cooling, step is as follows: adopt airless injection water smoke to carry out instantaneous temperature reduction, water temperature divides three sections, first paragraph water temperature is at 60-80 DEG C and spray 2-5min, and second segment water temperature is at 10-30 DEG C and spray 5-10min, and the 3rd section of water temperature is at 5-8 DEG C and spray 5-10min, water can cyclically utilizing, and vacuum tightness remains on-0.02-0.06MPa.
3. a PVC/PVF coextrusion tubing, is characterized in that, is made up of the raw material of following weight part:
4. PVC/PVF coextrusion tubing according to claim 3, is characterized in that, described polyvinyl chloride resin is SG-5 type resin.
5. PVC/PVF coextrusion tubing according to claim 3, is characterized in that, described stablizer is lead salt stabilizer, tin salt stabilizer, calcium zinc stabilizer, rare-earth stabilizer.
6. PVC/PVF coextrusion tubing according to claim 5, is characterized in that, described stablizer is calcium zinc stabilizer.
7. PVC/PVF coextrusion tubing according to claim 3, is characterized in that, described titanium dioxide is Rutile type Titanium Dioxide or anatase thpe white powder.
8. prepare a method for PVC/PVF coextrusion tubing according to claim 3, it is characterized in that comprising the following steps:
(1) prepare burden: weigh various raw material by proportioning;
(2) batch mixing: polyvinyl chloride resin, fine particle calcium carbonate, stablizer, SX630, stearic acid, paraffin and titanium dioxide are put into high low speed mixer and is uniformly mixed, rotating speed is 1000-2000RPM, mixing time is 10-20 minute, when being mixed to temperature 110-120 DEG C, material is put in low speed mixer, rotating speed 400-500RPM, to be mixedly obtains mixture to temperature 40-50 DEG C of discharging;
(3) double-layer coextrusion: mixture and PVF resin are dropped into respectively in twin screw unit or twin screw two-shipper hopper, add hot-extrudable after, shaping and export by double-layer coextrusion composite die, feeding rotating speed 10-40RPM, engine speed 30-150RPM, barrel zone temperature 150-200 DEG C, head temperature is 150-205 DEG C;
(4) Vacuum shaping cooling: adopt airless injection water smoke to carry out instantaneous temperature reduction, water temperature divides three sections, first paragraph water temperature is at 60-80 DEG C and spray 2-5min, second segment water temperature is at 10-30 DEG C and spray 5-10min, 3rd section of water temperature is at 5-8 DEG C and spray 5-10min, water can cyclically utilizing, and vacuum tightness remains on-0.02-0.06MPa;
(5) draw, cutting, obtains PVC/PVF coextrusion tubing.
9. the method preparing PVC/PVF coextrusion tubing according to claim 8, is characterized in that, the skin of described PVC/PVF coextrusion tubing is layer of PVC, and internal layer is PVF layer; Or skin is PVF layer, internal layer is layer of PVC.
10. the method preparing PVC/PVF coextrusion tubing according to claim 8, is characterized in that, PVF resin layer is 10-20 μm.
CN201510908748.6A 2015-12-09 2015-12-09 A kind of PVC/PVF coextrusion tubing and preparation method thereof Active CN105385063B (en)