CN105298133A - Construction method to strengthen crack resistance of large-volume concrete baseplate - Google Patents

Construction method to strengthen crack resistance of large-volume concrete baseplate Download PDF

Info

Publication number
CN105298133A
CN105298133A CN201510671215.0A CN201510671215A CN105298133A CN 105298133 A CN105298133 A CN 105298133A CN 201510671215 A CN201510671215 A CN 201510671215A CN 105298133 A CN105298133 A CN 105298133A
Authority
CN
China
Prior art keywords
concrete
crack
curing
conservation
construction method
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201510671215.0A
Other languages
Chinese (zh)
Other versions
CN105298133B (en
Inventor
韩锡云
袁志刚
许洵嘉
张瑶
徐文
张守治
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Know (suzhou) Prospective Design Consultant Co Ltd
Original Assignee
Know (suzhou) Prospective Design Consultant Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Know (suzhou) Prospective Design Consultant Co Ltd filed Critical Know (suzhou) Prospective Design Consultant Co Ltd
Priority to CN201510671215.0A priority Critical patent/CN105298133B/en
Publication of CN105298133A publication Critical patent/CN105298133A/en
Application granted granted Critical
Publication of CN105298133B publication Critical patent/CN105298133B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides a construction method to strengthen crack resistance of a large-volume concrete baseplate, which effectively controls generation of cracks of the large-volume concrete baseplate during a construction period. The construction method comprises pouring of a concrete cushion, layout of a slide layer, pouring of anti-crack concrete, conservation at a concrete plasticity stage and conservation at a concrete hardening stage, wherein the slide layer is constituted of two layers of plastic thin films between which a mixed fine material layer is sandwiched; a 7d restrained expansion rate in water conservation of the anti-crack concrete is not less than 0.02%, and a 28 d restrained expansion rate in the water conservation is not less than 0.03%; during the conservation at the concrete plasticity stage, a moisture evaporation inhibitor is sprayed after the pouring of the anti-crack concrete, plastering construction is started for one time after drying of the concrete surface, the moisture evaporation inhibitor is sprayed once again after the plastering, and the second time of plastering polishing processing is carried out 2 h before final setting; and during the conservation at the concrete hardening stage, a conservation agent is sprayed after hardening of the anti-crack concrete, the concrete is then covered by a layer of polystyrene board for thermal-preservation conservation, and a conservation period is not be less than 14 days.

Description

Construction method for improving crack resistance of large-volume concrete bottom plate
Technical Field
The invention relates to a foundation slab concrete construction method, in particular to a construction method for improving the crack resistance of a large-volume concrete slab.
Background
At present, with rapid development of economy and improvement of science and technology, building engineering is developed to be ultra-large and multifunctional, some ultra-block building structures are continuously generated, large-volume concrete is more and more applied to engineering, and ultra-long and ultra-large-volume concrete bottom plate foundations are increasingly increased. Because the base plate foundation is overlong and over-thick, and because the geological stress conditions of the foundation are different, the difficulty of the concrete crack control technology is increased, and the problem of the crack of the concrete structure of the base plate is a quite common quality problem. How to inhibit the cracking risk of large-volume floor concrete is the subject of the extensive engineering technical personnel at present.
Ultra-long and ultra-large (i.e. length over 60mm and area over 3600 m)2) The foundation slab is used as mass concrete and has the characteristics of large volume, complex engineering conditions and the like, cracking is easy to generate under the superposition effect of temperature stress and shrinkage stress, in order to avoid cracking, the main measures of the prior mass concrete slab crack control include that the central temperature of the concrete is reduced by adopting layering and sectional pouring, a post-cast strip is arranged to prevent the structure from shrinking and cracking, but the construction scheme brings certain trouble to the structural design and construction, and the defects that the post-cast strip can be poured after the structures on two sides are constructed for 60 days in the ⑴ design, the total construction period is prolonged, the template turnover is slow, the construction management cost is increased, the post-cast strip needs to be protected after the concrete is poured on two sides, the basement is always in a water leakage state before the post-cast strip is poured, the post-cast strip is filled with various sewage and construction wastes, the cleaning work is difficult, the soil body needs to be subjected to long-time dewatering treatment, the post-cast strip slab has the potential safety construction of anti-floating for a long time, the gaps between the post-cast strip and the post-cast strip can not be easily caused by the sealing stress at intervals, the pre-cast strip can cause serious tension stress when the post-cast construction process is kept, and the post-cast strip can be difficult to cause serious contradiction the post-cast stress retention of the post-cast construction process.
The technology of compensating the shrinkage concrete is developed according to a series of problems existing in the post-cast strip construction process. Under the condition that the reinforcement ratio is 0.2% -0.8%, the continuous pouring of the large-volume concrete bottom plate is realized by adopting the compensation shrinkage concrete and arranging one expansion reinforcing band every 30-40 m and combining the compensation shrinkage concrete and the expansion reinforcing band. Because the expansion agent used in the current market has the contradiction of inconsistent expansion development process and modern concrete contraction development process, the expansion agent has insufficient compensation contraction capability and limited capability of reducing the cracking risk of concrete.
The cracking of the cast-in-place large-volume concrete bottom plate is caused by single factors such as environmental temperature and humidity change, but is formed by the combined action of multiple factors. Such as, structural design aspects: the sliding layer is unreasonable in design, weak in sliding capacity and large in foundation constraint, so that the risk of confined cracking of the bottom plate concrete is increased; raw materials and mixing ratio: the mixing proportion of concrete is unreasonable, the hydration temperature is increased, the temperature difference between the inside and the outside is large, the shrinkage deformation is obvious, and the risk of shrinkage cracking of the concrete is aggravated; in the aspect of the construction process: the working performance and the maintenance scheme of the concrete are unreasonable during pouring, and the risk of cracking the concrete surface layer of the bottom plate is increased.
Disclosure of Invention
Object of the Invention
The invention aims to provide a construction method for improving the crack resistance of a large-volume concrete bottom plate, which effectively controls the generation of cracks in the construction period of the large-volume concrete bottom plate through the comprehensive application of various technologies.
The construction method for improving the crack resistance of the large-volume concrete bottom plate comprises the steps of pouring a concrete cushion layer, paving a sliding layer, pouring crack-resistant concrete, curing at the concrete plasticity stage and curing at the concrete hardening stage, wherein,
the sliding layer is formed by sandwiching a mixed fine material layer between two layers of plastic films, and the mixed fine material layer is prepared by uniformly mixing raw materials which comprise 20-30 parts of fly ash, 70-80 parts of talcum powder and 25-30 parts of water by mass;
the expansion rate of the crack-resistant concrete is limited by water curing for 7d and is not less than 0.02 percent, and the expansion rate of the crack-resistant concrete is limited by water curing for 28d and is not less than 0.03 percent and is not more than 0.04 percent;
the curing of the concrete shaping stage is to spray a moisture evaporation inhibitor immediately after the anti-crack concrete is poured, start primary plastering construction after the concrete surface is dried, spray the moisture evaporation inhibitor again after primary plastering, and perform secondary plastering and polishing treatment 2 hours before final setting;
and in the curing stage of the concrete, curing agent is sprayed immediately after the anti-crack concrete is cured, and then a layer of polystyrene board is covered for heat preservation and curing, wherein the curing period is not less than 14 days.
Preferably, the anti-crack concrete comprises the following components in percentage by mass:
the cement is 42.5-grade ordinary portland cement;
the fly ash is I-grade fly ash which meets the standard GB1596-2005 fly ash for cement and concrete;
the expanding agent is formed by compounding a calcium oxide expanding agent and a magnesium oxide expanding agent according to the mass ratio of (5-6) to (4-5), wherein the content of free calcium oxide (f-CaO) in the calcium oxide expanding agent is not less than 60%, and the active reaction time of the magnesium oxide expanding agent is 100-150 s;
the water reducing agent is a polycarboxylic acid water reducing agent with the water reducing rate of 25-30%;
the coarse aggregate is basalt macadam with the stacking porosity of 35-40%, and the mud content is controlled within 1%;
the fine aggregate is natural river sand with fineness modulus of 2.5-2.8, and the mud content is controlled within 1%.
Preferably, the mold-entering temperature of the anti-crack concrete is not higher than 20 ℃, and the slump is 16-18 cm.
Preferably, the thickness of the polyphenyl plate is 8-12 cm.
Preferably, the cushion layer is made of C15 plain concrete and has the thickness of 40-50 mm.
Preferably, the thickness of the sliding layer is 10-15 mm, and the tensile strength of the plastic film is 25-30 MPa.
The talcum powder, the calcium oxide expanding agent, the magnesium oxide expanding agent, the polycarboxylic acid water reducing agent, the polyphenyl board, the moisture evaporation inhibitor and the curing agent are all common materials known in the field, and commercially available products meeting requirements can be directly selected. The fineness of the talcum powder is preferably 300-500 meshes. The water evaporation inhibitor and the curing agent are sprayed by conventional dosage.
The existing large-volume concrete has low water-cement ratio and large using amount of cementing materials, has larger self-shrinkage, drying shrinkage and temperature reduction shrinkage than the traditional concrete, and the large-volume concrete bottom plate is easy to crack due to the superposition of shrinkage and the enlargement of one-time construction pouring length and area. Therefore, the applicant believes that the key to improving the crack resistance of the mass concrete floor is to reduce the constraint stress of the foundation to the concrete floor through reasonable sliding layer design, compensate the self-shrinkage and the temperature-drop shrinkage in the early and middle and later stages through effective expansion, and inhibit the plastic shrinkage, the drying shrinkage and the temperature-drop shrinkage through combined curing technology.
The invention finds that the fly ash and talcum powder slurry has small friction coefficient, convenient spraying construction and good laying uniformity through experimental research, can be used as a filling material of a sliding layer, and is beneficial to reducing the binding force between a foundation and a structural bottom plate.
The invention also finds that the calcium oxide expanding agent has high hydration reaction speed under normal temperature, can exert great expansion efficiency in the early stage (about 1-3 d), is very favorable for compensating the self-contraction in the early stage, and can generate great expansion in the early stage within a small mixing amount range. However, since the hydration reaction is rapid and the exothermic amount is high, the effect on the self-contraction and temperature-drop contraction of the long-term is not obvious.
The invention also finds that the magnesium oxide expanding agent prepared by calcining at the temperature of 900-1000 ℃ and with the active reaction time of 100-150s can generate larger expansion in the middle and later stages (3-28d) of hydration, particularly can generate effective expansion in the temperature reduction stage of concrete, and is beneficial to compensating the self-contraction and the temperature reduction contraction of the concrete in the middle and later stages. However, because of its relatively slow hydration reaction, the compensating effect on early self-shrinkage and drying shrinkage of concrete is very limited.
The invention also finds that the large-dosage fly ash can reduce the hydration temperature rise of the concrete, reduce the concentrated heat release phenomenon of the concrete and gain time for the slow heat dissipation of the concrete through experimental research; on the other hand, the expansion effect of the calcium oxide expanding agent and the magnesium oxide expanding agent can be increased, the expansion process of the expanding agent can be optimized by compounding and double-doping the calcium oxide expanding agent and the magnesium oxide expanding agent, and the crack resistance of the concrete is improved.
The invention also finds that the combined use of the moisture evaporation inhibitor, the curing agent and the polystyrene board can reduce the early and middle-stage moisture evaporation of the concrete, slow down the heat dissipation rate of the concrete, ensure the hydration water and the hydration temperature of the composite expanding agent, and is beneficial to improving the compensation effect of the calcium oxide expanding agent on the early self-shrinkage of the concrete and the compensation effect of the magnesium oxide expanding agent on the temperature-drop shrinkage of the concrete.
The technical principle of the invention is as follows: the problem that the dry-mixed mixture is difficult to lay uniformly in the prior sliding layer technology is solved by using the fly ash and talcum powder slurry as the sliding layer mixture; the novel anti-crack concrete is prepared by the calcium-magnesium composite expanding agent and the large-dosage fly ash double-dosage technology, on one hand, the hydration temperature rise of the concrete is regulated and controlled, the temperature concentration is reduced, the time is gained for the self heat dissipation of the concrete, on the other hand, the expansion development process of the expanding agent is regulated and controlled, the early expansion compensation concrete early drying and self-shrinkage can be generated, the effective expansion can be generated in the temperature reduction stage, the temperature shrinkage of the concrete is compensated, the temperature stress of the concrete is reduced, and meanwhile, when the large-dosage fly ash and the composite expanding agent are used in a double-dosage mode, the expansion process of the expanding agent can be optimized, the expansion effectiveness of the expanding agent is increased, and therefore, the anti-crack performance of the concrete; through the combined curing mode of the moisture evaporation inhibitor, the curing agent and the polystyrene board, on one hand, moisture evaporation is reduced, plastic shrinkage and drying shrinkage of concrete are inhibited, on the other hand, the heat dissipation speed of the concrete is slowed down, the phenomenon of temperature stress concentration is avoided, the temperature drop cracking risk of the concrete is reduced, meanwhile, through the combined curing mode, hydration water and hydration temperature of the composite expanding agent are ensured, the early expansion effect of the expanding agent and the expansion effect in the temperature drop stage are improved, and the effectiveness of expansion is improved.
Compared with the prior art, the invention has the outstanding advantages and effects that: by laying the novel sliding layer, the constraint of the foundation to the structural bottom plate is greatly reduced, so that the shrinkage stress in the structural bottom plate is reduced, the stress concentration caused by the constraint of the overlong and oversized concrete bottom plate due to self shrinkage is avoided, and the constraint cracking risk of the structural bottom plate can be effectively reduced; by doping the high-quality composite expanding agent, the expansion development process of the concrete is adjusted, and the drying shrinkage and self-shrinkage of the overlong and overlarge-volume bottom plate concrete are effectively compensated; the hydration process of the concrete is optimized and the temperature stress of the concrete is reduced by the aid of the large-amount fly ash and the control of the mold-entering temperature of the concrete, and the temperature crack of the concrete is effectively controlled by the aid of the heat-dissipation rate of the concrete slowed down by the aid of the covering of the heat-insulation boards; by spraying a water evaporation inhibitor, the plastic shrinkage crack of the concrete is effectively controlled; through spouting the curing agent, reduce the concrete top layer on the one hand and lose water dry, on the other hand has promoted the performance of compound expanding agent expansion efficiency, has effectively controlled the shrinkage crack of concrete. Through the comprehensive application of the technology, the generation of cracks in the construction period of the ultra-long and ultra-large volume concrete base plate foundation is effectively controlled, so that the construction quality meets the engineering requirements.
Drawings
FIG. 1 is a flow chart of a construction method for improving crack resistance of a large-volume concrete bottom plate.
Detailed Description
The invention is described in further detail below with reference to the drawings.
The materials selected in the following examples are as follows:
the cement is P.O42.5 cement produced by Anhui conch cement GmbH;
the fly ash is grade I fly ash produced by a Huaneng thermal power plant;
the talcum powder is produced by Nanjing Conlon stone powder Limited company and has the fineness of 400 meshes;
the plastic film is a polyvinyl chloride plastic film produced by Nanjing plastic factory, and the tensile strength is 27 MPa;
the water reducing agent is produced by Jiangsu Subot new material company LimitedA polycarboxylic acid high-performance water reducing agent;
the calcium oxide expanding agent is calcium oxide expanding agent with f-CaO content of 70% produced by Jiangsu Subo new materials GmbH;
the magnesium oxide expanding agent is prepared from 100s of magnesium oxide expanding agent with activity reaction time produced by Jiangsu Subo New Material Co.Ltd;
the coarse aggregate is selected from basalt macadam with 39% of stacking porosity, and the mud content is less than 1%;
the fine aggregate is river sand with fineness modulus of 2.6, and the mud content is less than 1%;
the water evaporation inhibitor is prepared from Jiangsu Subot new material, produced by GmbH-101 plastic concreteA highly effective water evaporation inhibitor;
the curing agent is produced by Jiangsu Subot new material company LimitedA high performance concrete curing agent;
the polystyrene board is an XPS extrusion molding insulation board produced by a green energy insulation material factory in Jintan city, Jiangsu province, and the thickness of the XPS extrusion molding insulation board is 10 cm.
The test methods referred to in the examples are as follows:
the method for testing the active reaction time of the magnesium oxide comprises the following steps: the method is executed according to an activity reaction time measuring method of magnesium oxide in appendix A of technical Specification for hydraulic concrete blending magnesium oxide of standard DL/T5296-2013;
the concrete limited expansion rate test method is executed by referring to a concrete limited expansion and contraction test method doped with an expansion agent in appendix B of GB23439-2009 concrete expansion agent.
The underground space development engineering is an underground two-layer structure, the negative two-layer bottom plate is directly connected with a foundation base and is in a basic rectangular shape, the east-west direction length is 420m, the south-north direction length is 135m, the thickness of the bottom plate is 1.2m, and the total building area is about 53865m2Belongs to an ultra-long and ultra-large volume concrete structure. If no deformation joint is arranged in the concrete bottom plate structure with large length and area, the seamless length of the structure is far beyond the limit value of the existing specification, and the improvement of the crack resistance of the large-volume concrete bottom plate is a very challenging task. As shown in fig. 1, the construction method comprises the following steps:
firstly, pouring concrete cushion layer
And after the earthwork is leveled, a layer of plain concrete with the thickness of 40mm and the strength grade of C15 is poured to be used as a foundation cushion layer.
Secondly, laying a sliding layer
Before laying the sliding layer, clean the basic bed course surface that the construction was accomplished earlier, lay the polyethylene plastic film that a layer thickness is 0.25mm, tensile strength is 27MPa earlier on the basic bed course, spray the concentrated fly ash talcum powder slurry of mixing of a layer thickness for 10mm next, will ensure the homogeneity of fly ash talcum powder slurry spraying when guaranteeing the sliding layer thickness, wherein the quality of fly ash talcum powder slurry constitutes: 30 parts of fly ash, 70 parts of talcum powder and 30 parts of water. And covering a layer of polyethylene plastic film with the thickness of 0.25mm and the tensile strength of 27MPa on the sprayed fly ash talcum powder slurry in time, wherein the polyethylene plastic film is laid to be flat, and the seam of the film is welded by hot melting, so that the laid polyethylene plastic film is integral. Thereby forming a sliding layer on the upper surface of the foundation mat layer.
Third, rolling the steel reinforcement
And rolling the steel bar with the reinforcement ratio of 0.15 according to the design requirement.
Fourthly, selecting raw materials and preparing the anti-crack concrete
P.O42.5 cement produced by Anhui conch cement company Limited, I-grade fly ash produced by Huaneng thermal power plant, calcium-magnesium composite expanding agent (formed by compounding calcium oxide expanding agent and magnesium oxide expanding agent according to the mass ratio of 6: 4), basalt broken stone with the stacking porosity of 39% as coarse aggregate, river sand with the fineness modulus of 2.6 as fine aggregate (the mud content of the coarse aggregate and the fine aggregate is controlled within 1%), polycarboxylic acid water reducer with the water reduction rate of 25% and water are selected to prepare the anti-crack concrete, wherein the components are respectively as follows according to the parts by mass: 190 parts of cement, 190 parts of fly ash, 40 parts of an expanding agent, 730 parts of fine aggregate, 1100 parts of coarse aggregate, 160 parts of water and 2.2 parts of a water reducing agent.
The expansion rate of the crack-resistant concrete is limited to 0.025 percent by water curing for 7d and 0.038 percent by water curing for 28 d.
Fifthly, pouring anti-crack concrete
And (3) pouring the anti-crack concrete by adopting a continuous construction mode, controlling the temperature of the concrete entering a mould not to be higher than 20 ℃, and controlling the slump to be 16-18 cm.
Sixthly, curing at the concrete plasticity stage
And immediately spraying a water evaporation inhibitor after the anti-crack concrete is poured, starting primary plastering construction after the concrete surface is dried, spraying the water evaporation inhibitor again after primary plastering to reduce the water evaporation of the concrete surface layer and reduce the plastic cracking risk, and performing secondary plastering and polishing treatment 2h before final setting.
Wherein,the plastic concrete high-efficiency water evaporation inhibitor is sprayed by adopting a conventional dosage, and specifically comprises the following steps:the efficient water evaporation inhibitor for plastic concrete is diluted in the proportion ofWater is 1:4, and the amount of the water evaporation inhibitor diluent sprayed each time is as follows: 1 literSpraying the diluent for 5m2Anti-crack concrete.
Seventhly, curing in the hardening stage of concrete
And immediately spraying a curing agent after the final setting and hardening of the anti-crack concrete to prevent the surface layer of the concrete from drying and losing water to generate drying shrinkage cracks, wherein the spraying frequency of the curing agent can be selected according to the actual environmental condition in the specific construction process. Wherein,the high-performance concrete curing agent is sprayed according to the conventional dosage, and the amount of the curing agent sprayed each time is 250g/m2Anti-crack concrete.
Eighthly, curing the concrete at the cooling stage
After the curing agent is sprayed, covering a layer of polystyrene board with the thickness of 10cm on the surface layer of the concrete for heat preservation and curing, wherein the curing period is not less than 14 days, the heat dissipation rate of the concrete is slowed down, and the temperature shrinkage crack caused by overlarge temperature drop amplitude of the concrete is prevented.
As mentioned above, a layer of C15 plain concrete with a thickness of 40mm is poured as a foundation pad layer; secondly, a novel sliding layer is prepared by adopting fly ash and talcum powder slurry with small friction coefficient as a sliding layer filling material and a double-layer plastic film, the sliding principle is similar to the bearing rotation principle, the constraint of a foundation on a structural bottom plate is greatly reduced, the stress concentration of overlong and oversized-area bottom plate concrete can be effectively reduced, and the structural crack resistance is improved; P.O42.5 cement produced by Anhui conch cement company Limited, I-grade fly ash produced by Huaneng thermal power plant, calcium magnesium composite expanding agent (formed by compounding calcium oxide expanding agent and magnesium oxide expanding agent according to the mass ratio of 6: 4), basalt broken stone with the stacking porosity of 39%, river sand with the fineness modulus of 2.6, polycarboxylic acid water reducing agent with the water reducing rate of 25% and water are selected again to prepare the anti-crack concrete, the underwater curing of the anti-crack concrete is tested, the expansion rate is limited by 7d and is 0.025%, the underwater curing is 28d and is 0.038%, the expansion development process is matched with the concrete structure development process, and the drying shrinkage and the self-shrinkage of the floor concrete with the overlong and ultra-large volume are effectively compensated; the hydration process of the concrete is optimized, the concentrated heat release phenomenon of the concrete is reduced, time is saved for slow heat dissipation of the concrete, and the temperature crack of the concrete is effectively controlled by using the large-dosage fly ash and controlling the mold-entering temperature of the concrete; and finally, by the combined use of the water evaporation inhibitor, the curing agent, the insulation board and other curing technologies, the early and middle-stage water evaporation of the concrete is effectively controlled, the heat dissipation rate of the concrete is slowed down, the hydration water and the hydration temperature of the composite expanding agent are ensured, the early expansion effect and the expansion effect in the temperature reduction stage of the expanding agent are improved, and the crack resistance of the structural concrete is improved. The comprehensive application of the technologies realizes the construction of the negative two-layer bottom plate of the underground space development project without setting deformation joints. The super-long and super-large-volume concrete bottom plate is poured in 3-month and 5-month days 2012, the heat insulation plate is removed after the curing is finished in 3-month and 28-month 2012, and no visible cracks are found. At present, no crack is found after more than three years of use and operation.

Claims (6)

1. A construction method for improving the crack resistance of a large-volume concrete bottom plate comprises the steps of pouring a concrete cushion layer, paving a sliding layer, pouring crack-resistant concrete, curing at the concrete plasticity stage and curing at the concrete hardening stage, wherein,
the sliding layer is formed by sandwiching a mixed fine material layer between two layers of plastic films, and the mixed fine material layer is prepared by uniformly mixing raw materials which comprise 20-30 parts of fly ash, 70-80 parts of talcum powder and 25-30 parts of water by mass;
the expansion rate of the crack-resistant concrete is limited by water curing for 7d and is not less than 0.02 percent, and the expansion rate of the crack-resistant concrete is limited by water curing for 28d and is not less than 0.03 percent and is not more than 0.04 percent;
the curing of the concrete shaping stage is to spray a moisture evaporation inhibitor immediately after the anti-crack concrete is poured, start primary plastering construction after the concrete surface is dried, spray the moisture evaporation inhibitor again after primary plastering, and perform secondary plastering and polishing treatment 2 hours before final setting;
and in the curing stage of the concrete, curing agent is sprayed immediately after the anti-crack concrete is cured, and then a layer of polystyrene board is covered for heat preservation and curing, wherein the curing period is not less than 14 days.
2. The construction method for improving the crack resistance of the large-volume concrete bottom plate according to claim 1, wherein the mass composition of the crack-resistant concrete comprises:
the cement is 42.5-grade ordinary portland cement;
the fly ash is I-grade fly ash which meets the standard GB1596-2005 fly ash for cement and concrete;
the expanding agent is formed by compounding a calcium oxide expanding agent and a magnesium oxide expanding agent according to the mass ratio of (5-6) to (4-5), wherein the content of free calcium oxide in the calcium oxide expanding agent is not lower than 60%, and the active reaction time of the magnesium oxide expanding agent is 100-150 s;
the water reducing agent is a polycarboxylic acid water reducing agent with the water reducing rate of 25-30%;
the coarse aggregate is basalt macadam with the stacking porosity of 35-40%, and the mud content is controlled within 1%;
the fine aggregate is natural river sand with fineness modulus of 2.5-2.8, and the mud content is controlled within 1%.
3. The construction method for improving the crack resistance of the large-volume concrete bottom plate according to claim 2, wherein the mold-entering temperature of the crack-resistant concrete is not higher than 20 ℃, and the slump is 16-18 cm.
4. The construction method for improving the crack resistance of the large-volume concrete bottom plate according to any one of claims 1 to 3, wherein the thickness of the polyphenyl plate is 8-12 cm.
5. The construction method for improving the crack resistance of the large-volume concrete bottom plate according to any one of claims 1 to 3, wherein the cushion layer is made of C15 plain concrete and has a thickness of 40-50 mm.
6. The construction method for improving the crack resistance of the large-volume concrete bottom plate according to any one of claims 1 to 3, wherein the thickness of the sliding layer is 10-15 mm, and the tensile strength of the plastic film is 25-30 MPa.
CN201510671215.0A 2015-10-13 2015-10-13 Design and Construction Method of Improving the Crack Resistance of Mass Concrete Floor Active CN105298133B (en)