CN105215072A - Biconial thin-wall high intensity aluminum alloy part thermoplasticity rheological molding mould and method - Google Patents
Biconial thin-wall high intensity aluminum alloy part thermoplasticity rheological molding mould and method Download PDFInfo
- Publication number
- CN105215072A CN105215072A CN201510664902.XA CN201510664902A CN105215072A CN 105215072 A CN105215072 A CN 105215072A CN 201510664902 A CN201510664902 A CN 201510664902A CN 105215072 A CN105215072 A CN 105215072A
- Authority
- CN
- China
- Prior art keywords
- mold
- blank
- guide ring
- groove
- aluminum alloy
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Withdrawn
Abstract
本发明公开了一种双锥形薄壁高强度铝合金零件热塑性流变成形模具及方法,所述模具包括凹模座、导向套圈、盖板和凸模芯,所述凹模座的内部开有凹槽,所述凹槽由两部分构成,凹槽的下方为倒锥形,凹槽的上方为圆柱形,锥形的底部直径与圆柱形的直径相同,导向套圈位于凹模座的上方,导向套圈的内径与凹模座中圆柱形凹槽的内径相同,导向套圈的上方设置盖板,所述凸模芯可从盖板和导向套圈中穿过并能最终穿入到凹模座的凹槽中,本发明的模具结构简单易行,仅用一套模具就可成形出具有连续金属流线的锥形薄壁零件。
The invention discloses a thermoplastic rheological forming mold and method for a biconical thin-walled high-strength aluminum alloy part. The mold includes a die base, a guide ring, a cover plate and a punch core. There is a groove inside, the groove is composed of two parts, the bottom of the groove is an inverted cone, the top of the groove is cylindrical, the diameter of the bottom of the cone is the same as the diameter of the cylinder, and the guide ring is located in the die Above the seat, the inner diameter of the guide ring is the same as the inner diameter of the cylindrical groove in the die seat, and a cover plate is set above the guide ring, and the male mold core can pass through the cover plate and the guide ring and can finally Penetrating into the groove of the die seat, the mold structure of the present invention is simple and easy, and only one set of molds can form a tapered thin-walled part with continuous metal streamlines.
Description
技术领域technical field
本发明属于热塑性挤压成形领域,特别是一种双锥形薄壁高强度铝合金零件热塑性流变成形模具及方法。The invention belongs to the field of thermoplastic extrusion forming, in particular to a biconical thin-walled high-strength aluminum alloy part thermoplastic rheological forming die and method.
背景技术Background technique
锥形薄壁零件是指零件壁厚在1mm左右、直径大于60mm的外形及内腔呈锥形的一类零件,主要由机械切削加工方法成形,也有用旋压方法成形,但旋压锥形薄壁零件、尤其是双锥薄壁零件的工艺技术难度大,工业实际应用很少。机械切削加工方法制造锥形薄壁零件的材料利用率在5%以下,切削工作量大、生产周期长,导致生产成本高、生产效率低,且切削加工使金属内部流线不连续,产品的强度及刚度等性能下降,因此,双锥薄壁零件切削加工工艺是一种落后的零件成形工艺。Conical thin-walled parts refer to a type of parts with a wall thickness of about 1mm, a diameter greater than 60mm, and a tapered inner cavity. It is mainly formed by mechanical cutting and spinning methods, but the spinning cone Thin-walled parts, especially double-cone thin-walled parts, are technically difficult, and there are few practical industrial applications. The material utilization rate of the tapered thin-walled parts manufactured by the mechanical cutting method is below 5%. The cutting workload is large and the production cycle is long, resulting in high production costs and low production efficiency. Moreover, the cutting process makes the internal streamline of the metal discontinuous, and the product quality The properties such as strength and stiffness are reduced. Therefore, the cutting process of double-cone thin-walled parts is a backward part forming process.
已有很多研究和专利用来克服上述不足。在《5A06铝合金非对称件双向加压拉深成形研究》的文献中,针对5A06铝合金非对称筒形零件所提出的用双向加压拉深法成形该零件,但成形件尺寸精度低;改用冷挤压后两次变薄拉伸成形工艺,提高了生产率,但加工余量大、产品合格率低。There have been many studies and patents to overcome the above-mentioned shortcomings. In the literature of "Research on Two-way Pressure Deep Drawing Forming of 5A06 Aluminum Alloy Asymmetric Parts", it is proposed to form the part by two-way pressure deep drawing method for 5A06 aluminum alloy asymmetric cylindrical parts, but the dimensional accuracy of the formed parts is low; Changing to the twice-thinning stretch forming process after cold extrusion improves the productivity, but the processing allowance is large and the product qualification rate is low.
专利号为200810232984.0的专利公开了一种高强度铝合金锥形薄壁件冷挤压成形工艺,该工艺的步骤包括:对棒材机加下料、挤压前退火处理和表面氧化及润滑处理、正挤压整形、一次挤锥孔、二次挤锥孔、固溶处理、时效处理,机加工外形,但是因其工序复杂、模具磨损大等原因而无法用于工业生产。Patent No. 200810232984.0 discloses a cold extrusion forming process for high-strength aluminum alloy conical thin-walled parts. The steps of the process include: feeding and blanking the bar, annealing before extrusion, surface oxidation and lubrication. , Positive extrusion shaping, primary extrusion cone hole, secondary extrusion cone hole, solution treatment, aging treatment, machining shape, but it cannot be used in industrial production due to its complicated process and large mold wear.
专利号为201410634255.3的专利公开了一种铝合金双锥异形深孔件毛坯挤压成型方法,具体为:将棒料切成节料;将节料放入加热炉中加热,温度达到300±20℃,并保温15min~20min;制作第一挤压模具、第二挤压模具、第三挤压模具和第四挤压模具,将第一、第二、第三挤压模具温度分别预热到250-300℃;分别在第一、第二、第三、第四挤压模具中,进行第一、第二、第三、第四次挤压,最后得到双锥异形深孔件毛坯,该件专利中成形需要4套模具,增加了实际生产的工艺复杂性。The patent No. 201410634255.3 discloses a method for extrusion molding of aluminum alloy double-cone special-shaped deep-hole blanks. ℃, and keep warm for 15min to 20min; make the first extrusion die, the second extrusion die, the third extrusion die and the fourth extrusion die, and preheat the temperature of the first, second and third extrusion dies to 250-300°C; In the first, second, third, and fourth extrusion dies, the first, second, third, and fourth extrusions are carried out, and finally the blank of the double-cone special-shaped deep hole is obtained. 4 sets of molds are required for forming in the piece patent, which increases the complexity of the actual production process.
由上可知,现有技术中尚无一种简单实用的生产双锥形薄壁高强度铝合金零件的模具和方法。It can be seen from the above that there is no simple and practical mold and method for producing biconical thin-walled high-strength aluminum alloy parts in the prior art.
发明内容Contents of the invention
本发明所解决的技术问题在于提供一种双锥形薄壁高强度铝合金零件热塑性流变成形模具及方法。The technical problem to be solved by the present invention is to provide a thermoplastic rheological forming mold and method for biconical thin-walled high-strength aluminum alloy parts.
实现本发明目的的技术解决方案为:一种双锥形薄壁高强度铝合金零件热塑性流变成形模具,包括凹模座、导向套圈、盖板和凸模芯,所述凹模座的内部开有凹槽,所述凹槽由两部分构成,凹槽的下方为倒锥形,凹槽的上方为圆柱形,锥形的底部直径与圆柱形的直径相同,导向套圈位于凹模座的上方,导向套圈的内径与凹模座中圆柱形凹槽的内径相同,导向套圈的上方设置盖板,所述凸模芯可从盖板和导向套圈中穿过并能最终穿入到凹模座的凹槽中,凸模芯外形与凹模座凹槽内形之间间隙为零件毛坯的壁厚。The technical solution for realizing the object of the present invention is: a kind of thermoplastic rheological forming mold of double-conical thin-walled high-strength aluminum alloy parts, comprising a die base, a guide ring, a cover plate and a punch core, the die base There is a groove inside, the groove is composed of two parts, the bottom of the groove is an inverted cone, the top of the groove is cylindrical, the diameter of the bottom of the cone is the same as the diameter of the cylinder, and the guide ring is located in the concave Above the mold base, the inner diameter of the guide ring is the same as the inner diameter of the cylindrical groove in the die base, and a cover plate is arranged above the guide ring, and the male mold core can pass through the cover plate and the guide ring and can Finally, it penetrates into the groove of the die holder, and the gap between the shape of the punch core and the inner shape of the groove of the die holder is the wall thickness of the part blank.
一种双锥形薄壁高强度铝合金零件热塑性流变成形方法,包括以下步骤:A method for thermoplastic rheological forming of a biconical thin-walled high-strength aluminum alloy part, comprising the following steps:
步骤1、坯料准备,将金属管料或棒料进行切削加工,将其切削成成形坯料;Step 1, blank preparation, cutting the metal pipe or bar, and cutting it into a shaped blank;
步骤2、模块预热,将工作面已喷刷涂料的凹模座、导向套圈、盖板和凸模芯放入加热炉中进行预热,之后保温;Step 2. Module preheating, put the die base, guide ring, cover plate and punch core that have been sprayed with paint on the working surface into the heating furnace for preheating, and then keep warm;
步骤3、合模,将刷有涂料的坯料放入预热后的凹模座内,再将导向套圈、盖板依次置于凹模座上端面上,最后将凸模芯放于导向套圈内,完成合模过程;Step 3. Clamp the mold, put the blank painted with paint into the preheated die seat, then place the guide ring and cover plate on the upper end surface of the die seat in turn, and finally put the punch core on the guide sleeve In the circle, complete the mold clamping process;
步骤4、模具加热,将已合模的模具放入炉中加热,之后保温;Step 4, mold heating, put the clamped mold into the furnace for heating, and then keep it warm;
步骤5、压制成形,保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈,再用与压机动滑块相连的压头将凸模芯在导向套圈的引导下压入凹模座中,凸模芯达到设定位置后保压一定时间后完成成形过程;Step 5. Pressing and forming. After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core on the guide sleeve. Under the guidance of the ring, it is pressed into the die seat, and the punch core reaches the set position, and the pressure is maintained for a certain period of time to complete the forming process;
步骤6、脱模,先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈加压,使凸模芯从成形件中退出;再从凹模座取下盖板、导向套圈,最后取出成形零件毛坯;Step 6, demoulding, first use the press cylinder to jack up the mold, then use the support rod to support the mold and return to the cylinder, and then use the blank holder slider to pressurize the guide ring to make the punch core withdraw from the formed part ; Then remove the cover plate and guide ring from the die seat, and finally take out the blank of the formed part;
步骤7、对零件毛坯进行热处理;Step 7, heat treating the part blank;
步骤8、对零件毛坯进行切削精加工,获得零件。Step 8, cutting and finishing the part blank to obtain the part.
本发明与现有技术相比,其显著优点为:1)本发明的方法解决现有切削加工成形工艺中生产双锥薄壁零件所存在的问题,用本发明提供的工艺方法可高效生产出材料利用率高、切削加工量少的零件;2)本发明的模具结构简单易行,仅用一套模具就可成形出具有连续金属流线的锥形薄壁零件;比切削加工法节省金属材料达到80%以上,还节省了大量的机械切削加工工时,简化了生产工艺。Compared with the prior art, the present invention has the remarkable advantages as follows: 1) The method of the present invention solves the existing problems in the production of double-cone thin-walled parts in the existing cutting and forming process, and the process method provided by the present invention can efficiently produce Parts with high material utilization rate and less cutting amount; 2) The mold structure of the present invention is simple and easy, and only one set of molds can be used to form tapered thin-walled parts with continuous metal streamlines; compared with the cutting method, it saves metal The material reaches more than 80%, and also saves a lot of mechanical cutting man-hours, and simplifies the production process.
下面结合附图对本发明作进一步详细描述。The present invention will be described in further detail below in conjunction with the accompanying drawings.
附图说明Description of drawings
图1为坯料形状示意图。Figure 1 is a schematic diagram of the blank shape.
图2为模具示意图。Figure 2 is a schematic diagram of the mold.
图3为合模图。Figure 3 is a mold drawing.
图4为压制结束示意图。Figure 4 is a schematic diagram of the end of pressing.
具体实施方式detailed description
结合附图,本发明的一种双锥形薄壁高强度铝合金零件热塑性流变成形模具,包括凹模座2、导向套圈3、盖板4和凸模芯5,所述凹模座2的内部开有凹槽,所述凹槽由两部分构成,凹槽的下方为倒锥形,凹槽的上方为圆柱形,锥形的底部直径与圆柱形的直径相同,导向套圈3位于凹模座2的上方,导向套圈3的内径与凹模座2中圆柱形凹槽的内径相同,导向套圈3的上方设置盖板4,所述凸模芯5可从盖板4和导向套圈3中穿过并能最终穿入到凹模座2的凹槽中,凸模芯5外形与凹模座2凹槽内形之间间隙为零件毛坯的壁厚。In conjunction with the accompanying drawings, a thermoplastic rheological forming mold for a biconical thin-walled high-strength aluminum alloy part of the present invention includes a die base 2, a guide ring 3, a cover plate 4 and a punch core 5, the die There is a groove inside the seat 2, the groove is composed of two parts, the bottom of the groove is an inverted cone, the top of the groove is cylindrical, the diameter of the bottom of the cone is the same as that of the cylinder, and the guide collar 3 is located above the die base 2, the inner diameter of the guide collar 3 is the same as the inner diameter of the cylindrical groove in the die base 2, a cover plate 4 is arranged above the guide collar 3, and the punch core 5 can be removed from the cover plate 4 and the guide collar 3 pass through and can finally penetrate into the groove of the die holder 2, and the gap between the outer shape of the punch core 5 and the inner shape of the groove of the die holder 2 is the wall thickness of the part blank.
一种基于上述模具的双锥形薄壁高强度铝合金零件热塑性流变成形方法,包括以下步骤:A method for thermoplastic rheological forming of biconical thin-walled high-strength aluminum alloy parts based on the above mold, comprising the following steps:
步骤1、坯料准备,将金属管料或棒料进行切削加工,将其切削成成形坯料1;Step 1, blank preparation, cutting the metal tube or bar, and cutting it into a forming blank 1;
步骤2、模块预热,将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4和凸模芯5放入加热炉中进行预热,之后保温;所述涂料为:水基石墨涂料。预热温度为430℃~500℃,保温时间为40min~80min。Step 2, module preheating, put the die base 2, the guide ring 3, the cover plate 4 and the punch core 5 that have been sprayed with paint on the working surface into the heating furnace for preheating, and then keep warm; the paint is: Water-based graphite paint. The preheating temperature is 430°C-500°C, and the holding time is 40min-80min.
步骤3、合模,将刷有涂料的坯料1放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;所述涂料为:水基石墨涂料。Step 3, mold closing, put the blank 1 brushed with paint into the preheated die base 2, then place the guide ring 3 and cover plate 4 on the upper end surface of the die base 2 in sequence, and finally place the punch The core 5 is placed in the guide ring 3 to complete the mold clamping process; the coating is: water-based graphite coating.
步骤4、模具加热,将已合模的模具放入炉中加热,之后保温;加热温度为430℃~500℃,保温20min~60min。Step 4, mold heating, put the clamped mold into the furnace for heating, and then keep warm; the heating temperature is 430°C-500°C, keep warm for 20min-60min.
步骤5、压制成形,保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到设定位置后保压一定时间后完成成形过程;保压的时间为8~15秒。Step 5. Pressing and forming. After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the Guided by the guide ring 3, it is pressed into the die base 2, and the punch core 5 reaches the set position, and the pressure is kept for a certain period of time to complete the forming process; the time for keeping the pressure is 8 to 15 seconds.
步骤6、脱模,先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈4加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;Step 6, demoulding, first use the press jacking cylinder to jack up the mold, then support the mold with a support rod and then return to the jacking cylinder, and then use the blank holder slider to pressurize the guide ring 4, so that the punch core 5 can be lifted from the formed part Then withdraw from the die base 2; then remove the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the blank 6 of the formed part;
步骤7、对零件毛坯6进行热处理;Step 7, heat-treating the part blank 6;
步骤8、对零件毛坯6进行切削精加工,获得零件。Step 8, cutting and finishing the part blank 6 to obtain the part.
下面结合实施例进行更详细的描述:Below in conjunction with embodiment carry out more detailed description:
实施例1Example 1
最大外径80mm、壁厚5mm、第一锥为40度、第二锥为9度、总145mm的双锥形2A12铝合金零件的热塑性流变成形工艺如下:The thermoplastic rheological forming process of a biconical 2A12 aluminum alloy part with a maximum outer diameter of 80 mm, a wall thickness of 5 mm, a first cone of 40 degrees, a second cone of 9 degrees, and a total of 145 mm is as follows:
⑴备坯料1:先将双锥形2A12铝合金零件图转化为内外表面加工余量分别为0.5mm、0.6mm的成形毛坯图,再根据毛坯件的重量、形状结构特点,确定坯料[1]的形状和尺寸,最后选用2A12铝合金管料外径为55mm、壁厚10mm经切削加工成一端内、外径为54mm、36mm,另一端内、外径为48mm、38mm,总长为115mm的(所有尺寸公差≤0.10mm)成形坯料1;⑴Blank preparation 1: first convert the biconical 2A12 aluminum alloy part drawing into a forming blank drawing with a machining allowance of 0.5mm and 0.6mm on the inner and outer surfaces, and then determine the blank according to the weight, shape and structural characteristics of the blank[1] Finally, the 2A12 aluminum alloy pipe material with an outer diameter of 55mm and a wall thickness of 10mm is selected and processed into one end with an inner and outer diameter of 54mm and 36mm, and the other end with an inner and outer diameter of 48mm and 38mm, and a total length of 115mm ( All dimensional tolerances ≤0.10mm) forming blank 1;
⑵模块预热:将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4、凸模芯5放入加热炉中预热,加热温度为470℃±3℃,保温60min;(2) Module preheating: Put the die base 2, guide ring 3, cover plate 4, and punch core 5 that have been sprayed with paint on the working surface to preheat in a heating furnace. ;
⑶合模:将刷有涂料的坯料1按小端向下的方向放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;(3) Mold closing: put the blank 1 brushed with paint into the preheated die base 2 in the direction of the small end downward, and then place the guide ring 3 and cover plate 4 on the upper end surface of the die base 2 in sequence , and finally put the punch core 5 in the guide ring 3 to complete the mold clamping process;
⑷模具加热:将已合模的模具放入炉中加热,加热温度为460℃±3℃,保温30min;⑷Mould heating: Put the closed mold into the furnace to heat, the heating temperature is 460℃±3℃, keep it warm for 30min;
⑸压制成形:保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到一定位置后保压10秒后完成成形过程;(5) Compression forming: After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the guide sleeve Under the guidance of the ring 3, press it into the die seat 2, and the punch core 5 reaches a certain position, and the pressure is kept for 10 seconds to complete the forming process;
⑹脱模:先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈4加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;⑹Demoulding: first use the press cylinder to jack up the mold, then use the support rod to support the mold and then return to the cylinder, and then use the blank holder slider to pressurize the guide ring 4 to make the punch core 5 withdraw from the formed part ; Then take off the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the formed part blank 6;
⑺热处理:对零件毛坯6进行如下热处理,具体的热处理工艺由零件毛坯6的材料类型确定;⑺Heat treatment: perform the following heat treatment on the part blank 6, and the specific heat treatment process is determined by the material type of the part blank 6;
⑻精加工:按零件图要求对零件毛坯6进行切削加工,获得形状、尺寸与力学性能均满足要求的零件。⑻Finishing: According to the requirements of the part drawing, the part blank 6 is cut and processed to obtain parts that meet the requirements in shape, size and mechanical properties.
实施例2Example 2
直线段长33mm、外径为115mm,第二锥为28度,壁厚均为5mm、总长为215mm的双锥形2A12铝合金零件的热塑性流变成形工艺如下:The thermoplastic rheological forming process of a biconical 2A12 aluminum alloy part with a length of 33 mm, an outer diameter of 115 mm, a second cone of 28 degrees, a wall thickness of 5 mm, and a total length of 215 mm is as follows:
⑴坯料1:先将双锥形2A12铝合金零件图转化为内、外表面加工余量分别为1.0mm、0.8mm的成形毛坯图,由该毛坯件的重量、形状,确定所用坯料1的形状和尺寸,最后选用2A12铝合金管料外径为80mm、壁厚10mm、长度为120mm,一端的外侧倒角为4×28°、另一端的内侧倒角为4×28°,总长为120mm的(所有尺寸公差≤0.10mm)成形坯料1;⑴Blank 1: first convert the biconical 2A12 aluminum alloy part drawing into a forming blank drawing with machining allowances of 1.0mm and 0.8mm on the inner and outer surfaces respectively, and determine the shape of the blank 1 used by the weight and shape of the blank And size, finally choose 2A12 aluminum alloy pipe material with outer diameter of 80mm, wall thickness of 10mm, length of 120mm, the outer chamfer of one end is 4×28°, the inner chamfer of the other end is 4×28°, and the total length is 120mm (All dimensional tolerances ≤0.10mm) Formed blank 1;
⑵模块预热:将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4、凸模芯5放入加热炉中预热,加热温度为490℃±3℃,保温60min;(2) Module preheating: put the die base 2, guide ring 3, cover plate 4, and punch core 5 that have been sprayed with paint on the working surface to preheat in a heating furnace. ;
⑶合模:将内外表面刷有涂料的坯料1按外侧倒角端向下的方向放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;(3) Clamping the mold: Put the blank 1 painted with paint on the inner and outer surfaces into the preheated die seat 2 in the direction of the outer chamfered end downward, and then place the guide ring 3 and the cover plate 4 in the die seat in sequence 2 On the upper end face, finally put the punch core 5 in the guide ring 3 to complete the mold clamping process;
⑷模具加热:将已合模的模具放入炉中加热,加热温度为480℃±3℃,保温40min;⑷Mould heating: Put the closed mold into the furnace to heat, the heating temperature is 480℃±3℃, keep it warm for 40min;
⑸压制成形:保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到一定位置后保压13秒后完成成形过程;(5) Compression forming: After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the guide sleeve Under the guidance of the ring 3, press it into the die seat 2, and the punch core 5 reaches a certain position, and the pressure is maintained for 13 seconds to complete the forming process;
⑹脱模:先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈3加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;⑹Demoulding: first use the press jacking cylinder to jack up the mold, then support the mold with a support rod and return to the jacking cylinder, and then use the blank holder slider to pressurize the guide ring 3 to make the punch core 5 withdraw from the formed part ; Then take off the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the formed part blank 6;
⑺热处理:对零件毛坯6进行如下热处理,具体的热处理工艺由零件毛坯6的材料类型确定;⑺Heat treatment: perform the following heat treatment on the part blank 6, and the specific heat treatment process is determined by the material type of the part blank 6;
⑻精加工:按零件图要求对零件毛坯6进行切削加工,获得形状、尺寸与力学性能均满足要求的零件。⑻Finishing: According to the requirements of the part drawing, the part blank 6 is cut and processed to obtain parts that meet the requirements in shape, size and mechanical properties.
实施例3Example 3
最大外径80mm、壁厚5mm、第一锥为40度、第二锥为9度、总145mm的双锥形2A12铝合金零件的热塑性流变成形工艺如下:The thermoplastic rheological forming process of a biconical 2A12 aluminum alloy part with a maximum outer diameter of 80 mm, a wall thickness of 5 mm, a first cone of 40 degrees, a second cone of 9 degrees, and a total of 145 mm is as follows:
⑴坯料1:先将双锥形2A12铝合金零件图转化为内、外表面加工余量分别为1.0mm、0.8mm的成形毛坯图,由该毛坯件的重量、形状,确定所用坯料1的形状和尺寸,最后选用2A12铝合金管料外径为80mm、壁厚10mm、长度为120mm,一端的外侧倒角为4×28°、另一端的内侧倒角为4×28°,总长为120mm的(所有尺寸公差≤0.10mm)成形坯料1;⑴Blank 1: first convert the biconical 2A12 aluminum alloy part drawing into a forming blank drawing with machining allowances of 1.0mm and 0.8mm on the inner and outer surfaces respectively, and determine the shape of the blank 1 used by the weight and shape of the blank And size, finally choose 2A12 aluminum alloy pipe material with outer diameter of 80mm, wall thickness of 10mm, length of 120mm, the outer chamfer of one end is 4×28°, the inner chamfer of the other end is 4×28°, and the total length is 120mm (All dimensional tolerances ≤0.10mm) Formed blank 1;
⑵模块预热:将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4、凸模芯5放入加热炉中预热,加热温度为430℃,保温40min;(2) Module preheating: Put the die base 2, guide ring 3, cover plate 4, and punch core 5 that have been sprayed with paint on the working surface into the heating furnace for preheating. The heating temperature is 430°C and the heat preservation time is 40 minutes;
⑶合模:将内外表面刷有涂料的坯料1按外侧倒角端向下的方向放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;(3) Clamping the mold: Put the blank 1 painted with paint on the inner and outer surfaces into the preheated die seat 2 in the direction of the outer chamfered end downward, and then place the guide ring 3 and the cover plate 4 in the die seat in sequence 2 On the upper end face, finally put the punch core 5 in the guide ring 3 to complete the mold clamping process;
⑷模具加热:将已合模的模具放入炉中加热,加热温度为430℃,保温20min;⑷Mould heating: put the closed mold into the furnace to heat, the heating temperature is 430°C, keep it warm for 20min;
⑸压制成形:保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到一定位置后保压8秒后完成成形过程;(5) Compression forming: After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the guide sleeve Under the guidance of the ring 3, press it into the die base 2, and the punch core 5 reaches a certain position, and the pressure is maintained for 8 seconds to complete the forming process;
⑹脱模:先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈3加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;⑹Demoulding: first use the press jacking cylinder to jack up the mold, then support the mold with a support rod and return to the jacking cylinder, and then use the blank holder slider to pressurize the guide ring 3 to make the punch core 5 withdraw from the formed part ; Then take off the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the formed part blank 6;
⑺热处理:对零件毛坯6进行如下热处理,具体的热处理工艺由零件毛坯6的材料类型确定;⑺Heat treatment: perform the following heat treatment on the part blank 6, and the specific heat treatment process is determined by the material type of the part blank 6;
⑻精加工:按零件图要求对零件毛坯6进行切削加工,获得形状、尺寸与力学性能均满足要求的零件。⑻Finishing: According to the requirements of the part drawing, the part blank 6 is cut and processed to obtain parts that meet the requirements in shape, size and mechanical properties.
实施例4Example 4
最大外径80mm、壁厚5mm、第一锥为40度、第二锥为9度、总145mm的双锥形2A12铝合金零件的热塑性流变成形工艺如下:The thermoplastic rheological forming process of a biconical 2A12 aluminum alloy part with a maximum outer diameter of 80 mm, a wall thickness of 5 mm, a first cone of 40 degrees, a second cone of 9 degrees, and a total of 145 mm is as follows:
⑴坯料1:先将双锥形2A12铝合金零件图转化为内、外表面加工余量分别为1.0mm、0.8mm的成形毛坯图,由该毛坯件的重量、形状,确定所用坯料1的形状和尺寸,最后选用2A12铝合金管料外径为80mm、壁厚10mm、长度为120mm,一端的外侧倒角为4×28°、另一端的内侧倒角为4×28°,总长为120mm的(所有尺寸公差≤0.10mm)成形坯料1;⑴Blank 1: first convert the biconical 2A12 aluminum alloy part drawing into a forming blank drawing with machining allowances of 1.0mm and 0.8mm on the inner and outer surfaces respectively, and determine the shape of the blank 1 used by the weight and shape of the blank And size, finally choose 2A12 aluminum alloy pipe material with outer diameter of 80mm, wall thickness of 10mm, length of 120mm, the outer chamfer of one end is 4×28°, the inner chamfer of the other end is 4×28°, and the total length is 120mm (All dimensional tolerances ≤0.10mm) Formed blank 1;
⑵模块预热:将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4、凸模芯5放入加热炉中预热,加热温度为500℃,保温80min;(2) Module preheating: Put the die base 2, guide ring 3, cover plate 4, and punch core 5 that have been sprayed with paint on the working surface into the heating furnace for preheating. The heating temperature is 500°C and the heat preservation time is 80 minutes;
⑶合模:将内外表面刷有涂料的坯料1按外侧倒角端向下的方向放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;(3) Clamping the mold: Put the blank 1 painted with paint on the inner and outer surfaces into the preheated die seat 2 in the direction of the outer chamfered end downward, and then place the guide ring 3 and the cover plate 4 in the die seat in sequence 2 On the upper end face, finally put the punch core 5 in the guide ring 3 to complete the mold clamping process;
⑷模具加热:将已合模的模具放入炉中加热,加热温度为500℃,保温60min;⑷Mould heating: put the closed mold into the furnace to heat, the heating temperature is 500℃, and keep it warm for 60min;
⑸压制成形:保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到一定位置后保压15秒后完成成形过程;(5) Compression forming: After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the guide sleeve Under the guidance of the ring 3, press it into the die seat 2, and the punch core 5 reaches a certain position, and the pressure is maintained for 15 seconds to complete the forming process;
⑹脱模:先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈3加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;⑹Demoulding: first use the press jacking cylinder to jack up the mold, then support the mold with a support rod and return to the jacking cylinder, and then use the blank holder slider to pressurize the guide ring 3 to make the punch core 5 withdraw from the formed part ; Then take off the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the formed part blank 6;
⑺热处理:对零件毛坯6进行如下热处理,具体的热处理工艺由零件毛坯6的材料类型确定;⑺Heat treatment: perform the following heat treatment on the part blank 6, and the specific heat treatment process is determined by the material type of the part blank 6;
⑻精加工:按零件图要求对零件毛坯6进行切削加工,获得形状、尺寸与力学性能均满足要求的零件。⑻Finishing: According to the requirements of the part drawing, the part blank 6 is cut and processed to obtain parts that meet the requirements in shape, size and mechanical properties.
实施例5Example 5
直线段长33mm、外径为115mm,第二锥为28度,壁厚均为5mm、总长为215mm的双锥形2A12铝合金零件的热塑性流变成形工艺如下:The thermoplastic rheological forming process of a biconical 2A12 aluminum alloy part with a length of 33 mm, an outer diameter of 115 mm, a second cone of 28 degrees, a wall thickness of 5 mm, and a total length of 215 mm is as follows:
⑴坯料1:先将双锥形2A12铝合金零件图转化为内、外表面加工余量分别为1.0mm、0.8mm的成形毛坯图,由该毛坯件的重量、形状,确定所用坯料1的形状和尺寸,最后选用2A12铝合金管料外径为80mm、壁厚10mm、长度为120mm,一端的外侧倒角为4×28°、另一端的内侧倒角为4×28°,总长为120mm的(所有尺寸公差≤0.10mm)成形坯料1;⑴Blank 1: first convert the biconical 2A12 aluminum alloy part drawing into a forming blank drawing with machining allowances of 1.0mm and 0.8mm on the inner and outer surfaces respectively, and determine the shape of the blank 1 used by the weight and shape of the blank And size, finally choose 2A12 aluminum alloy pipe material with outer diameter of 80mm, wall thickness of 10mm, length of 120mm, the outer chamfer of one end is 4×28°, the inner chamfer of the other end is 4×28°, and the total length is 120mm (All dimensional tolerances ≤0.10mm) Formed blank 1;
⑵模块预热:将工作面已喷刷涂料的凹模座2、导向套圈3、盖板4、凸模芯5放入加热炉中预热,加热温度为460℃±3℃,保温60min;(2) Module preheating: Put the die base 2, guide ring 3, cover plate 4, and punch core 5 that have been sprayed with paint on the working surface to preheat in a heating furnace. ;
⑶合模:将内外表面刷有涂料的坯料1按外侧倒角端向下的方向放入预热后的凹模座2内,再将导向套圈3、盖板4依次置于凹模座2上端面上,最后将凸模芯5放于导向套圈3内,完成合模过程;(3) Clamping the mold: Put the blank 1 painted with paint on the inner and outer surfaces into the preheated die seat 2 in the direction of the outer chamfered end downward, and then place the guide ring 3 and the cover plate 4 in the die seat in sequence 2 On the upper end face, finally put the punch core 5 in the guide ring 3 to complete the mold clamping process;
⑷模具加热:将已合模的模具放入炉中加热,加热温度为480℃±3℃,保温40min;⑷Mould heating: Put the closed mold into the furnace to heat, the heating temperature is 480℃±3℃, keep it warm for 40min;
⑸压制成形:保温完成后,将模具移到四柱油压机工作台面上,先用压边滑块压紧导向套圈3,再用与压机动滑块相连的压头将凸模芯5在导向套圈3的引导下压入凹模座2中,凸模芯5达到一定位置后保压13秒后完成成形过程;(5) Compression forming: After the heat preservation is completed, move the mold to the working table of the four-column hydraulic press, first press the guide ring 3 with the blank holder slider, and then use the pressure head connected to the press motor slider to place the punch core 5 on the guide sleeve Under the guidance of the ring 3, press it into the die seat 2, and the punch core 5 reaches a certain position, and the pressure is maintained for 13 seconds to complete the forming process;
⑹脱模:先用压机顶缸顶起模具,再用撑杆支撑住模具后退回顶缸,然后用压边滑块对导向套圈3加压,使凸模芯5从成形件中退出;再从凹模座2取下盖板4、导向套圈3,最后取出成形零件毛坯6;⑹Demoulding: first use the press jacking cylinder to jack up the mold, then support the mold with a support rod and return to the jacking cylinder, and then use the blank holder slider to pressurize the guide ring 3 to make the punch core 5 withdraw from the formed part ; Then take off the cover plate 4 and the guide ring 3 from the die base 2, and finally take out the formed part blank 6;
⑺热处理:对零件毛坯6进行如下热处理,具体的热处理工艺由零件毛坯6的材料类型确定;⑺Heat treatment: perform the following heat treatment on the part blank 6, and the specific heat treatment process is determined by the material type of the part blank 6;
⑻精加工:按零件图要求对零件毛坯6进行切削加工,获得形状、尺寸与力学性能均满足要求的零件。⑻Finishing: According to the requirements of the part drawing, the part blank 6 is cut and processed to obtain parts that meet the requirements in shape, size and mechanical properties.
本发明通过选用合适的原材料形状与尺寸,用1套模具即可成形出双锥形薄壁毛坯件,再经少量的机械切削加工,获得双锥形薄壁零件。本发明的模具结构简单易行;比切削加工法节省金属材料达到80%以上,还节省了大量的机械切削加工工时,简化了生产工艺。In the present invention, by selecting suitable shapes and sizes of raw materials, a biconical thin-walled blank can be formed with a set of molds, and then a biconical thin-walled part can be obtained through a small amount of mechanical cutting. The mold structure of the invention is simple and easy to implement; compared with the cutting method, the metal material can be saved by more than 80%, and a large amount of mechanical cutting working hours can be saved, and the production process is simplified.
Claims (6)