CN104057665B - Glass fibre composite fire-proof laminate - Google Patents
Glass fibre composite fire-proof laminate Download PDFInfo
- Publication number
- CN104057665B CN104057665B CN201410230474.5A CN201410230474A CN104057665B CN 104057665 B CN104057665 B CN 104057665B CN 201410230474 A CN201410230474 A CN 201410230474A CN 104057665 B CN104057665 B CN 104057665B
- Authority
- CN
- China
- Prior art keywords
- glass fibre
- pressing
- temperature
- composite fire
- minute
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The present invention relates to glass fibre composite fire-proof laminate, by glass fibre mat after impregnating resin slurry, through the glass fibre mat being compounded with solidification coating that high temperature drying, pressing are formed;The formula of described resin slurry is phenol 10.5% 12.5%, formaldehyde 12.5% 15.5%, ethanol 10% 13%, ammonia 0.3% 1%, Caustic soda 0.5% 1%, calcium carbonate or calcium oxide 46% 54%, aluminium hydroxide or aluminium oxide 5% 8%, softening agent 4% 5%.The characteristic of glass fibre and resin is combined by the present invention, has fire prevention, good waterproof performance, intensity corruption high, anti-, the advantages such as heat insulation, sound-proofing is good.
Description
Technical field
The present invention relates to glass fibre composite fire-proof laminate, for construction and decoration field.
Background technology
The most traditional product uses wood pulp paper impregnating resin, by the interior decoration surfacing formed after high temperature high pressure process, it has light weight, mildew-resistant, fire prevention, performance heat-resisting, antidetonation, easy to clean are widely used, in addition to solid wood furniture, the plate fitment of all kinds of top grades has the participation of melamine plate.Adding the problem of environmental pollution that above-mentioned interior decoration surfacing can effectively prevent the formaldehyde used as preservative and Lauxite from being brought in the integral wardrobe of middle and high end, the most this interior decoration surfacing also replaces wood-based planet, aluminium-plastic panel etc. and makes the facings such as minute surface, high abrasion, antistatic, embossment, metal.But papery fire-proof board there is also some problems, as poor in flameproof effect, water resistance is poor, matter is crisp, intensity is low and affects its application performance.
Summary of the invention
In order to overcome drawbacks described above, it is an object of the invention to provide a kind of glass fibre composite fire-proof laminate, use glass dipping technique and hot extrusion briquetting technique, the characteristic of glass fibre and resin is combined, there is fire prevention, good waterproof performance, intensity corruption high, anti-, the advantages such as heat insulation, sound-proofing is good.
To achieve these goals, the invention provides a kind of glass fibre composite fire-proof laminate, by glass fibre mat after impregnating resin slurry, through the glass fibre mat being compounded with solidification coating that high temperature drying, pressing are formed;The formula of described resin slurry is phenol 10.5%-12.5%, formaldehyde 12.5%-15.5%, ethanol 10%-13%, ammonia 0.3%-1%, Caustic soda 0.5%-1%, calcium carbonate or calcium oxide 46%-54%, aluminium hydroxide or aluminium oxide 5%-8%, softening agent 4%-5%.
As a further improvement on the present invention: the preparation process of described resin slurry is:
A, take the phenol of 50%-75%, formaldehyde melt after add reactor together with ammonia, start stirring simultaneously, in 15-25min, be warming up to 55-60 DEG C, keep 15-25min;
B, the speed of 10 DEG C of heating up with every 15 minutes are warming up to 70-90 DEG C, react at this temperature;
After muddiness occurs in solution in c, question response still, maintain the temperature at 75-85 DEG C, after 50-60 minute, add residue phenol, formaldehyde, and add Caustic soda;After above-mentioned material adds, heat up in 15-20min and control temperature at 75-85 DEG C;
In d, question response still, there is muddiness and again after 20 minutes in solution, observes and is repeatedly detected solution and reach 52-67*10 in viscosity-6Ethanol is added after/S index;
E, maintain the temperature at 75-85 DEG C, after 25-35 minute, be cooled to less than 35 DEG C, close stirring blanking;
F, before impregnation technology, calcium carbonate or calcium oxide, aluminium hydroxide or aluminium oxide and softening agent and above-mentioned material are mixed to form resin slurry.
As the preferred embodiments of the present invention: described concentration of alcohol is more than 95%.
As the preferred embodiments of the present invention: described ammonia is strong aqua ammonia.
As a further improvement on the present invention: a diameter of 6-16um of glass fibre in described glass fibre mat, the glass fibre of the most a length of 6-10 um accounts for 25-50%, the glass fibre of a length of 10-16um accounts for 50-75%.So collocation of glass fiber diameter thickness ensures the compactness in felt face, prevents the absorption glue that glass fibre mat is too much.
As a further improvement on the present invention: on the one hand in order to ensure the intensity in dipping process, on the other hand in order to ensure the intensity of finished product and reduce the cold and hot contraction caused by variations in temperature, keeping the stability of product, the glass fibre in described glass fibre mat is arranged in pairs or groups by the glass fibre of the glass fibre of a length of 6-12mm of 25-40%, a length of 16-32mm of 60-75% and is formed.
As a further improvement on the present invention: the high temperature of described resin slurry is dried particularly as follows: use low early and high after cascade raising temperature subregion baking and curing technique, and temperature is cascade raising temperature between 100-140 DEG C.The temperature being so possible to prevent front road too high makes resin premature cure, causes and occurs in finished product that shrinkage cavity, surface are grown dim phenomenon thus affected the quality of product.
As a further improvement on the present invention: the present invention according to different pressing-in temp, time, pressure and the parameters of different thickness designs, particularly as follows:
A: product thickness is 0.5-0.8mm, and pressing pressure is 12-13
Mpa, pressing-in temp is 100-120 DEG C, and hot pressing time is 8-12 minute;
B: product thickness is 0.8-1.2mm, and pressing pressure is 13-15
Mpa, pressing-in temp is 110-125 DEG C, and hot pressing time is 12-20 minute;
C: product thickness is 1.2-2.0mm, and pressing pressure is 15-18Mpa, and pressing-in temp is 115-130 DEG C, and hot pressing time is 18-25 minute;
D: product thickness is 2.0-3.0mm, and pressing pressure is 18-25Mpa, and pressing-in temp is 120-135 DEG C, and hot pressing time is 22-30 minute;
E: product thickness is 3.0-6.0mm, and pressing pressure is 25-35Mpa, and pressing-in temp is 135-155 DEG C, and hot pressing time is 30-40 minute.
It is an advantage of the current invention that:
1, the present invention uses glass fibre mat as substrate, has saved timber resources, and can recycle, beneficially environmental protection.
2, the present invention uses glass fibre mat as substrate, after impregnating resin slurry, through High Temperature High Pressure molding, has heatproof high, do not fire, anti-corruption compared with organic fiber, heat insulation, sound-proofing good, and tensile strength is high, the features such as electrical insulating property is good.
3, the present invention had both had the pliability of organic board, can re-workability, there is again the fire prevention of inorganic plate, resistance to water, and intensity be higher than any dalle, be the energy-conservation ideal material of novel building.
4, glass fibre composite fire-proof laminate of the present invention uses with no paper veneer, enhance fire resistance and heat-insulating property, its fire protecting performance is much better than the material such as paper dalle, wood based panel, can be widely applied to need the place of protection against the tide, mildew-resistant, fire prevention and high intensity, as used on interior wall, ceiling, exterior wall, roof, it is particularly suitable for the extra high occasions of fire protection requirement such as toilet, kitchen, general merchandise store, place of public amusement and uses.
Detailed description of the invention
Below in conjunction with the embodiment of the present invention, the technical scheme in the embodiment of the present invention is clearly and completely described, it is clear that described embodiment is only a part of embodiment of the present invention rather than whole embodiments.Based on the embodiment in the present invention, the every other embodiment that those of ordinary skill in the art are obtained under not making creative work premise, broadly fall into the scope of protection of the invention.
Embodiment 1, the preparation of glass fibre composite fire-proof laminate:
The preparation of glass fibre mat: with glass fibre as raw material, preferably diameter 6um, a length of 8mm and a diameter of 14um, the alkali-free glass fibre of a length of 25mm mix by weight 1:2, glass fibre mat is made according to maturation process, ensure that dense uniform and the production efficiency of glass mat, testing its grammes per square metre is 80g/, and combustible content is 18% ± 2%, and tension force is 10kg-20kg, hot strength is longitudinal 200N, horizontal 100N.
Configuration resin slurry 1000kg, operates as follows: weigh phenol 120kg, Liquid for maldehyde 146kg, high purity ethanol 120kg, and concentration is the ammonia 6kg of 30%, Caustic soda 8kg, calcium carbonate 500kg, aluminium oxide 60kg, resin softening agent 40kg;
Take the phenol of 80kg, formaldehyde adds reactor after melting together with ammonia, starts stirring at low speed simultaneously, is warming up to 56 DEG C in 18min, keeps 18min;Being warming up to 80 DEG C with the speed of intensification in every 15 minutes 10 DEG C again, material carries out chemical reaction at this temperature;
After muddiness occurs in solution in question response still, maintain the temperature at 80 DEG C, after 60 minutes, add remaining 40kg phenol and 68kg formaldehyde, and add Caustic soda;Heat up in 18min and control temperature at 80 DEG C;
In question response still, there is muddiness and again after 20 minutes in solution, observes and is repeatedly detected solution and reach 55*10 in viscosity-6Ethanol is added after the index of/S;Maintain the temperature at 80 DEG C, after 30 minutes, be cooled to less than 35 DEG C, close stirring blanking;Calcium carbonate or calcium oxide, aluminium hydroxide or aluminium oxide and softening agent are mixed to form resin slurry with above-mentioned blanking.
Impregnation technology: controlling at 40-60% according to control of product impregnation resin content glass mat spread of 80g/ in prescribed limit, this enforcement of different grammes per square metre glass fibre belts and customer requirement different-thickness, solvent volatile quantity controls at 3-5%;The controlling of spread ensure the uniform distribution in glass mat of glue in dipping process and control pressing after the thickness of product.Excessive glue is easily produced during the too high pressing of spread;Too low bond when causing product pressing insecure.The control of solvent volatile quantity ensures product resin mobility inside base material in pressing process, if solvent volatile quantity is higher, may cause having occurred in bonding processes the phenomenons such as bag, layering;If solvent volatile quantity is on the low side, then when being likely to result in hot pressing surface can not well moistening and produce blowing phenomenon.
Stoving process: baking and curing process is divided into five regions to carry out, the temperature in first and secondth district is 110 DEG C, 120 DEG C, third and fourth, 5th district be 120 DEG C, 130 DEG C, 140 DEG C.
In this enforcement, speed of production is 40m/min, and it is adjusted according to glass fibre mat thickness, it is ensured that after dipping, product surface resin is uniform curing.
Process for pressing: simultaneously carry out pressing drying, according to pressing-in temp, time, pressure and parameters that different thickness designs is different, table 1 is as follows:
| Product specification | Pressure (Mpa) | Temperature (DEG C) | Hot pressing time (min) | Temperature retention time (min) | Chilling temperature |
| 0.5-0.8mm | 12-13 | 100-120 | 8-12 | 15 | Less than 35 DEG C |
| 0.8-1.2mm | 13-15 | 110-125 | 12-20 | 20 | Less than 40 DEG C |
| 1.2-2.0mm | 15-18 | 115-130 | 18-25 | 20 | Less than 50 DEG C |
| 2.0-3.0mm | 18-25 | 120-135 | 30 | 30 | Less than 50 DEG C |
| 3.0-6.0mm | 25-35 | 135-155 | 40 | 40 | Less than 50 DEG C |
In this step, the pressure of heat pressing process, temperature and hot pressing time three elements are mutual dependence for existence, again mutually restriction, and three factors are different on the impact of thick china.
The chemical reaction of impregnating resin is mainly played catalytic action by hot pressing temperature, i.e. accelerating solidification, temperature height is conducive to the demoulding after overlaying, and can shorten pressing cycle, improve yield, but too high temperature makes resin have little time Uniform Flow i.e. to be solidified, and causes plate face to have micro-pore.Easily rebound and rough in plate face.
Pressure can ensure that combination good between base material, under suitable temperature and pressure effect, after impregnating the resin melting in paper, solidification, forms closing, fine and close surface, it is also possible to make the most gentle micro-pore of substrate surface be filled.On the premise of not affecting product quality, low pressure should be used as far as possible, but the adhesion strength of too low pressure influence base material and dipping paper and resin fluid ability.
The length of hot pressing time depends on curing rate and the hot pressing temperature of impregnating resin, and overlong time can cause resin over cure, loses due elasticity, crackle, warpage occurs easily to product in the course of processing;Time is too short, and resin solidification is inadequate, easily produces haftplatte phenomenon, the physicochemical property of impact, the ruggedness of product.
This product is after impregnating, adding hot pressing, and product has the performance of common papery PLASTIC LAMINATED, and after testing, its flame retardant rating can reach A level, and oxygen index (OI) reaches 60, than common fire prevention one grade of plate hight.80 DEG C of hot-water soaks do not have obvious tympanites phenomenon for 72 hours, and water resistance is substantially better than papery plate.During construction and decoration, the nail-holding ability due to glass fibre composite fire-proof laminate is strong, can directly on sheet material boring install and without as tradition PLASTIC LAMINATED on body of wall mounting framework, therefore construction is simply, fast, improves efficiency of construction.
Embodiment 2, the preparation of glass fibre composite fire-proof laminate:
The preparation of glass fibre mat: with glass fibre as raw material, preferably diameter 8um, a length of 11mm and a diameter of 15um, the alkali-free glass fibre of a length of 27mm mix by weight 1:2.5, glass fibre mat is made according to maturation process, ensure that dense uniform and the production efficiency of glass mat, testing its grammes per square metre is 110g/, tension force is 18kg, and hot strength is longitudinal 210N, horizontal 120N.
Configuration resin slurry 1000kg, operates as follows: weigh phenol 110kg, Liquid for maldehyde 130kg, high purity ethanol 110kg, and concentration is the ammonia 10kg of 30%, Caustic soda 10kg, calcium oxide 520kg, aluminium hydroxide 70kg, glass fibre softening agent 50kg;
Take the phenol of 80kg, 70kg formaldehyde adds reactor after melting together with ammonia, starts stirring at low speed simultaneously, is warming up to 58 DEG C in 20min, keeps 22min;Being warming up to 85 DEG C with the speed of intensification in every 15 minutes 10 DEG C again, material carries out chemical reaction at this temperature;
After muddiness occurs in solution in question response still, maintain the temperature at 80 DEG C, after 55 minutes, add remaining phenol and formaldehyde, and add Caustic soda;Heat up in 16min and control temperature at 82 DEG C;
In question response still, there is muddiness and again after 20 minutes in solution, observes and is repeatedly detected solution and reach 60*10 in viscosity-6Ethanol is added after the index of/S;Maintain the temperature at 82 DEG C, after 28 minutes, be cooled to less than 35 DEG C, close stirring blanking;Calcium carbonate or calcium oxide, aluminium hydroxide or aluminium oxide and softening agent are mixed to form resin slurry with above-mentioned blanking.
Impregnation technology: controlling at 50-80% according to control of product impregnation resin content glass mat spread of 110 g/ in prescribed limit, this enforcement of different grammes per square metre glass fibre belts and customer requirement different-thickness, solvent volatile quantity controls at 3-5%.
Stoving process: baking and curing process is divided into five regions to carry out, the temperature in first and secondth district is 110 DEG C, 110 DEG C, third and fourth, 5th district be 120 DEG C, 130 DEG C, 140 DEG C.
In this enforcement, speed of production is 30m/min, and it is adjusted according to glass fibre mat thickness, it is ensured that after dipping, product surface resin is uniform curing.
Process for pressing: according to the form in embodiment 1, select suitable pressing-in temp, time, pressure and parameters according to different thickness, carry out pressing drying simultaneously.
This product is through impregnating, add hot pressing aftershaping, and final product performance index test is as follows:
Claims (7)
1. a glass fibre composite fire-proof laminate, is characterized by: by glass fibre mat after impregnating resin slurry, through the glass fibre mat being compounded with solidification coating that high temperature drying, pressing are formed;The formula of described resin slurry is phenol 10.5%-12.5%, formaldehyde 2.5%-15.5%, ethanol 10%-13%, ammonia 0.3%-1%, Caustic soda 0.5%-1%, calcium carbonate or calcium oxide 46%-54%, aluminium hydroxide or aluminium oxide 5%-8%, softening agent 4%-5%, above each component sum is 100%;The preparation process of described resin slurry is:
A, take the phenol of 50%-75%, formaldehyde melt after add reactor together with ammonia, start stirring simultaneously, in 15-25min, be warming up to 55-60 DEG C, keep 15-25min;
B, the speed of 10 DEG C of heating up with every 15 minutes are warming up to 70-90 DEG C, react at this temperature;
After muddiness occurs in solution in c, question response still, maintain the temperature at 75-85 DEG C, after 50-60 minute, add residue phenol, formaldehyde, and add Caustic soda;After above-mentioned material adds, heat up in 15-20min and control temperature at 75-85 DEG C;
In d, question response still, there is muddiness and again after 20 minutes in solution, observes and is repeatedly detected solution and reach 52-67 × 10 in viscosity-6 Ethanol is added after/S index;
E, maintain the temperature at 75-85 DEG C, after 25-35 minute, be cooled to less than 35 DEG C, close stirring blanking;
F, before impregnation technology, calcium carbonate or calcium oxide, aluminium hydroxide or aluminium oxide and softening agent and above-mentioned material are mixed to form resin slurry.
Glass fibre composite fire-proof laminate the most according to claim 1, is characterized by: described concentration of alcohol is more than 95%.
Glass fibre composite fire-proof laminate the most according to claim 1, is characterized by: described ammonia is strong aqua ammonia.
Glass fibre composite fire-proof laminate the most according to claim 1, is characterized by: a diameter of 6-16 μm of glass fibre in described glass fibre mat.
Glass fibre composite fire-proof laminate the most according to claim 4, is characterized by: the glass fibre in described glass fibre mat is arranged in pairs or groups by the glass fibre of the glass fibre of a length of 6-10 μm of 25-50%, a length of 10-16 μm of 50-75% and formed.
6. according to the glass fibre composite fire-proof laminate described in claim 1, it is characterized by: the high temperature of described resin slurry is dried particularly as follows: use low early and high after cascade raising temperature subregion baking and curing technique, and temperature is cascade raising temperature between 100-140 DEG C.
7., according to the glass fibre composite fire-proof laminate described in claim 1, it is characterized by: described pressing particularly as follows:
A: product thickness is 0.5-0.8mm, and pressing pressure is 12-13 MPa, and pressing-in temp is 100-120 DEG C, and hot pressing time is 8-12 minute;
B: product thickness is 0.8-1.2mm, and pressing pressure is 13-15 MPa, and pressing-in temp is 110-125 DEG C, and hot pressing time is 12-20 minute;
C: product thickness is 1.2-2.0mm, and pressing pressure is 15-18 MPa, and pressing-in temp is 115-130 DEG C, and hot pressing time is 18-25 minute;
D: product thickness is 2.0-3.0mm, and pressing pressure is 18-25 MPa, and pressing-in temp is 120-135 DEG C, and hot pressing time is 22-30 minute;
E: product thickness is 3.0-6.0mm, and pressing pressure is 25-35 MPa, and pressing-in temp is 135-155 DEG C, and hot pressing time is 30-40 minute.