CN102982992B - A kind of preparation method of room temperature Wet-pressing molding anisotropic bonded NdFeB magnet - Google Patents
A kind of preparation method of room temperature Wet-pressing molding anisotropic bonded NdFeB magnet Download PDFInfo
- Publication number
- CN102982992B CN102982992B CN201210271255.2A CN201210271255A CN102982992B CN 102982992 B CN102982992 B CN 102982992B CN 201210271255 A CN201210271255 A CN 201210271255A CN 102982992 B CN102982992 B CN 102982992B
- Authority
- CN
- China
- Prior art keywords
- magnetic
- room temperature
- magnetic powder
- magnet
- anisotropic bonded
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
本发明属于磁性材料领域,具体涉及一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,包括磁粉表面改性工序、粘结剂与磁粉混合工序、磁粉浆料制备工序、磁场模压成型工序和真空固化工序几个工序,其中,所述的磁场模压成型工序中采用的成型方式为室温下湿压成型。本发明中,磁体的成型工序是在室温下进行,因此具有成型工艺简单、生产效率高、能耗低的优点,而且由于是湿压成型,磁粉颗粒之间存在一层液体薄膜,可有效降低磁粉颗粒取向时的摩擦阻力,提高磁体的磁性能。The invention belongs to the field of magnetic materials, and in particular relates to a method for preparing an anisotropically bonded NdFeB magnet by wet pressing at room temperature, including a magnetic powder surface modification process, a binder and magnetic powder mixing process, a magnetic powder slurry preparation process, and magnetic field compression molding process and vacuum curing process, wherein the forming method adopted in the magnetic field compression molding process is wet pressing at room temperature. In the present invention, the molding process of the magnet is carried out at room temperature, so it has the advantages of simple molding process, high production efficiency, and low energy consumption, and because it is wet pressing molding, there is a layer of liquid film between the magnetic powder particles, which can effectively reduce The friction resistance when the magnetic powder particles are oriented improves the magnetic properties of the magnet.
Description
技术领域 technical field
本发明属于磁性材料领域,具体涉及一种室温湿压成型各向异性粘结NdFeB磁体的制备方法。 The invention belongs to the field of magnetic materials, in particular to a method for preparing an anisotropic bonded NdFeB magnet formed by wet pressing at room temperature.
背景技术 Background technique
粘结NdFeB磁体因其具有尺寸精度高、形态自由度大、机械强度好、便于大批量生产等优点,广泛地应用于航天、交通、计算机、医疗等领域。目前,粘结NdFeB磁体大多为各向同性磁体,这类磁体的磁性能一般很低,限制了其进一步的应用与发展。因此,随着电子产品向轻、薄、微、小等微型化、形状复杂化发展,具有更高磁性能的各向异性粘结NdFeB磁体被人们寄予厚望。 Bonded NdFeB magnets are widely used in aerospace, transportation, computer, medical and other fields because of their advantages of high dimensional accuracy, large degree of shape freedom, good mechanical strength, and easy mass production. At present, most bonded NdFeB magnets are isotropic magnets, and the magnetic properties of such magnets are generally very low, which limits their further application and development. Therefore, with the development of miniaturization and complex shapes of electronic products such as light, thin, micro, and small, anisotropic bonded NdFeB magnets with higher magnetic properties are placed high expectations.
为了使各向异性粘结NdFeB磁体具有高磁性能,必须使磁体内部的磁粉定向排列,因此各向异性粘结NdFeB磁体一般需要在磁场下成型。早期的研究者们曾尝试采用室温磁场干压成形的方法制备各向异性粘结NdFeB磁体,如公开号为CN1087744 A的发明专利所述的用于生产各向异性粘结磁体的固体树脂及其制造方法:将各向异性粘结NdFeB磁粉与粘结剂混合搅拌后,采用球磨的方法裂化磁粉,然后在室温下进行磁场干压成型,这种方法虽然可以制备出各向异性粘结NdFeB磁体,但是,由于室温下磁粉表面的粘结剂为固态,磁粉之间的摩擦力很大,导致磁场下磁粉取向困难,因此很难制备出性能优异的各向异性粘结NdFeB磁体。后续的研究者又提出了磁场温压成型的方法, 如日本专利特开平8-31677号所述的磁各向异性树脂结合型磁体的制造方法:将各向异性粘结NdFeB磁粉与粘结剂混合搅拌,形成粘结剂涂敷的磁粉颗粒,然后将磁粉颗粒放入模具中加热,使粘结剂处于熔融状态,最后进行磁场取向,制备出高取向度的各向异性粘结NdFeB磁体,该方法解决了室温下磁粉颗粒之间摩擦力大,取向困难的问题,然而,由于加热状态下磁粉表面的粘结剂软化后易黏附在模具壁上,该方法也存在加料困难的问题。针对这一难题,公开号为CN1087744 A的发明专利提出了多步成型制造各向异性粘结NdFeB磁体的方法:将混合粘结剂后的磁粉先进行冷压成型,制备出密度较低的预压坯,然后将预压坯在磁场下温压成型,最后固化得到各向异性粘结NdFeB磁体,这一方法虽然解决了各向异性磁粉热状态下加料困难的问题,但是不可避免的增加了工艺难度,降低了生产效率。磁场湿压成型工艺作为一种制备各向异性磁体的有效工艺,在各向异性烧结铁氧体的生产中得到了广泛的应用,如公开号为CN101354939A的发明专利公开了一种超细永磁铁氧体二次成型浆料的制备方法,将该浆料进行磁场湿压成型后,进行烧结处理,可以制备出高性能的铁氧体永磁,但是,该方法却没有在各向异性粘结NdFeB磁体的成型上得到应用。 In order to make the anisotropic bonded NdFeB magnet have high magnetic properties, the magnetic powder inside the magnet must be aligned, so the anisotropic bonded NdFeB magnet generally needs to be formed under a magnetic field. Early researchers tried to prepare anisotropic bonded NdFeB magnets by dry pressing in a room temperature magnetic field, such as the solid resin used to produce anisotropic bonded magnets and its Manufacturing method: After mixing and stirring the anisotropic bonded NdFeB magnetic powder and the binder, the magnetic powder is cracked by ball milling, and then dry-pressed in a magnetic field at room temperature. Although this method can prepare anisotropic bonded NdFeB magnets However, since the binder on the surface of the magnetic powder is solid at room temperature, the friction between the magnetic powders is very large, resulting in difficulty in the orientation of the magnetic powder under a magnetic field, so it is difficult to prepare an anisotropic bonded NdFeB magnet with excellent performance. Subsequent researchers also proposed a method of magnetic field warm pressing molding, such as the manufacturing method of magnetic anisotropic resin-bonded magnets described in Japanese Patent Laid-Open No. 8-31677: anisotropic bonded NdFeB magnetic powder and binder Mix and stir to form binder-coated magnetic powder particles, and then put the magnetic powder particles into the mold to heat, so that the binder is in a molten state, and finally perform magnetic field orientation to prepare an anisotropic bonded NdFeB magnet with a high degree of orientation. This method solves the problem of high friction between magnetic powder particles and difficult orientation at room temperature. However, since the binder on the surface of the magnetic powder is softened and easily adheres to the mold wall under heating, this method also has the problem of difficult feeding. To solve this problem, the invention patent with the publication number CN1087744 A proposed a multi-step molding method to manufacture anisotropic bonded NdFeB magnets: the magnetic powder mixed with the binder was first cold-pressed to prepare a low-density pre-molded magnet. compaction, and then warm-press the preform under a magnetic field, and finally solidify to obtain an anisotropic bonded NdFeB magnet. Although this method solves the problem of difficult feeding of anisotropic magnetic powder in a hot state, it inevitably increases the Process difficulty reduces production efficiency. As an effective process for preparing anisotropic magnets, the magnetic field wet pressing process has been widely used in the production of anisotropic sintered ferrite. For example, the invention patent with the publication number CN101354939A discloses an ultra-fine permanent magnet The preparation method of the ferrite secondary molding slurry, after the slurry is wet-pressed in a magnetic field, and then sintered, a high-performance ferrite permanent magnet can be prepared, but this method does not have an anisotropic bonding It has been applied in the forming of NdFeB magnets.
发明内容 Contents of the invention
本发明针对现有各向异性粘结NdFeB磁体制备工艺复杂、生产效率低的不足,提供一种室温湿压成型各向异性粘结NdFeB磁体的制备方法。 The invention provides a method for preparing the anisotropic bonded NdFeB magnet by wet pressing at room temperature, aiming at the disadvantages of complex preparation process and low production efficiency of the existing anisotropic bonded NdFeB magnet.
本发明的目的是通过以下技术方案得以实施的: The purpose of the present invention is implemented through the following technical solutions:
一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,包括磁粉表面改性工序、粘结剂与磁粉混合工序、磁粉浆料制备工序、磁场模压成型工序和真空固化工序几个工序,其中,所述的磁场模压成型工序中采用的成型方式为室温下湿压成型。 A method for preparing an anisotropically bonded NdFeB magnet by wet pressing at room temperature, comprising several steps of magnetic powder surface modification, binder and magnetic powder mixing, magnetic powder slurry preparation, magnetic field compression molding, and vacuum curing, Wherein, the molding method adopted in the magnetic field compression molding process is wet compression molding at room temperature.
发明人发现,采用湿压成型工艺时,由于磁粉颗粒之间存在一层液态隔膜,有效地降低了取向时磁粉颗粒之间的摩擦力,从而有利于提高磁粉的取向度,使磁体具有优异的磁性能,而且,由于湿压成型工艺是在室温下进行,可避免出现温压成型工艺中加料困难的情况。 The inventors found that when using the wet pressing molding process, since there is a layer of liquid diaphragm between the magnetic powder particles, the friction force between the magnetic powder particles during orientation is effectively reduced, which is beneficial to improve the orientation degree of the magnetic powder and make the magnet have excellent Moreover, since the wet pressing process is carried out at room temperature, it can avoid the difficulty of feeding materials in the warm pressing process.
发明人还发现,在进行湿压成型步骤时,浆料中的溶剂在压制力的作用下可被挤出磁体,并不影响磁体的最终密度。 The inventors also found that during the wet pressing step, the solvent in the slurry can be squeezed out of the magnet under the action of the pressing force, without affecting the final density of the magnet.
作为优选,根据本发明所述的一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,其中,所述的磁场模压成型工序中采用的磁场强度为1-2T,压力为3-9t/m2。这么做是为了提高磁体中磁粉的取向度及磁体的密度,从而提高磁体的磁性能。 As a preference, according to a method for preparing an anisotropic bonded NdFeB magnet by wet pressing at room temperature according to the present invention, wherein the magnetic field strength used in the magnetic field compression molding process is 1-2T, and the pressure is 3-9t /m 2 . This is done to increase the degree of orientation of the magnetic powder in the magnet and the density of the magnet, thereby improving the magnetic properties of the magnet.
作为优选,根据本发明所述的一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,其中,所述的磁粉浆料制备工序中添加溶剂,所述的溶剂由甲醇、乙醇、水、磷酸溶液或矿物油中的一种或者几种组成。溶剂添加量控制在NdFeB磁粉质量的50%左右。 As a preference, according to the preparation method of anisotropic bonded NdFeB magnet formed by room temperature wet pressing according to the present invention, a solvent is added in the preparation process of the magnetic powder slurry, and the solvent is composed of methanol, ethanol, water , phosphoric acid solution or one or more of mineral oil. The amount of solvent added is controlled at about 50% of the mass of NdFeB magnetic powder.
作为优选,根据本发明所述的一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,其中,所述的磁粉浆料制备工序中添加表面活性剂,所述的表面活性剂由十二烷基苯磺酸钠、聚山梨酯、脂肪酸甘油酯、焦磷酸钠、三聚磷酸钠或偏磷酸钠中的一种或者几种组成。这么做是为了使团聚在一起的磁粉颗粒散开,并悬浮在溶剂中,形成磁粉浆料。表面活性剂的用量为NdFeB磁粉质量的0.1%~1%,用量太少无法使磁粉分散到溶剂中,形成均匀的磁粉浆料;用量太多则效果饱和,同时非磁性相增加影响磁体的磁性能。 As a preference, according to the preparation method of anisotropic bonded NdFeB magnet formed by room temperature wet pressing according to the present invention, a surfactant is added in the preparation process of the magnetic powder slurry, and the surfactant consists of ten One or more of sodium dialkylbenzenesulfonate, polysorbate, fatty acid glyceride, sodium pyrophosphate, sodium tripolyphosphate or sodium metaphosphate. This is done to disperse the agglomerated magnetic powder particles and suspend them in a solvent to form a magnetic powder slurry. The amount of surfactant used is 0.1% to 1% of the mass of NdFeB magnetic powder. If the amount is too small, the magnetic powder cannot be dispersed into the solvent to form a uniform magnetic powder slurry; if the amount is too large, the effect will be saturated, and the increase of non-magnetic phase will affect the magnetic properties of the magnet. able.
作为优选,根据本发明所述的一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,其中,所述的磁粉浆料制备工序中添加润滑剂,所述的润滑剂由硬脂酸锌、硬脂酸钙、PE腊、乙撑双硬脂酰胺或季戊四醇硬脂酸酯中的一种或者几种组成。这么做是为了降低磁粉取向时的摩擦阻力,提高取向度。润滑剂的添加量一般为NdFeB磁粉质量的0.1%~1%,低于0.1%则润滑效果偏弱,降低磁粉取向度,高于1%则润滑效果饱和,增加非磁性相含量降低磁体磁性能。 As a preference, according to the preparation method of anisotropic bonded NdFeB magnet formed by room temperature wet pressing according to the present invention, a lubricant is added in the preparation process of the magnetic powder slurry, and the lubricant is composed of stearic acid One or more of zinc, calcium stearate, PE wax, ethylene bisstearamide or pentaerythritol stearate. This is done in order to reduce the frictional resistance during magnetic powder orientation and increase the degree of orientation. The amount of lubricant added is generally 0.1% to 1% of the mass of NdFeB magnetic powder. If it is less than 0.1%, the lubricating effect will be weak and the orientation degree of the magnetic powder will be reduced. If it is higher than 1%, the lubricating effect will be saturated, and the increase in non-magnetic phase content will reduce the magnetic properties of the magnet. .
作为优选,根据本发明所述的一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,其中,所述的磁粉浆料制备工序中添加溶剂,并对磁粉及溶剂进行球磨,球磨时所采用的磨球密度为2-5g/cm3,如玻璃球、铝球、氧化铝球。球磨会使粘结剂与磁粉混合工序中粘在一起的磁粉发生裂解,形成单个的各向异性磁粉颗粒,可进一步提高磁体中磁粉的取向度。密度过低的磨球无法使磁粉颗粒裂解,而密度过高的磨球会导致磁粉组织被破坏,降低磁性能。 As a preference, according to a method for preparing an anisotropically bonded NdFeB magnet formed by room temperature wet pressing according to the present invention, wherein a solvent is added in the preparation process of the magnetic powder slurry, and the magnetic powder and the solvent are ball milled, during ball milling, The density of the grinding balls used is 2-5g/cm 3 , such as glass balls, aluminum balls, and alumina balls. Ball milling will crack the magnetic powder stuck together in the binder and magnetic powder mixing process to form a single anisotropic magnetic powder particle, which can further increase the orientation degree of the magnetic powder in the magnet. Grinding balls with too low density cannot crack the magnetic powder particles, while grinding balls with too high density will destroy the magnetic powder structure and reduce the magnetic performance.
与现有技术相比,本发明具有以下优点: Compared with the prior art, the present invention has the following advantages:
本发明中,磁体的成型工序是在室温下进行,因此具有成型工艺简单、生产效率高、能耗低的优点,而且由于是湿压成型,磁粉颗粒之间存在一层液体薄膜,可有效降低磁粉颗粒取向时的摩擦阻力,提高磁体的磁性能。 In the present invention, the molding process of the magnet is carried out at room temperature, so it has the advantages of simple molding process, high production efficiency, and low energy consumption, and because it is wet pressing molding, there is a layer of liquid film between the magnetic powder particles, which can effectively reduce The friction resistance when the magnetic powder particles are oriented improves the magnetic properties of the magnet.
具体实施方式 Detailed ways
下面结合实施例,更具体地说明本发明的内容。应当理解,本发明的实施并不局限于下面的实施例,对本发明所做的任何形式上的变通和/或改变都将落入本发明保护范围。 Below in conjunction with embodiment, the content of the present invention is described more specifically. It should be understood that the implementation of the present invention is not limited to the following examples, and any modifications and/or changes made to the present invention will fall within the protection scope of the present invention.
在本发明中,若非特指,所有的份、百分比均为重量单位,所有的设备和原料等均可从市场购得或是本行业常用的。下述实施例中的方法,如无特别说明,均为本领域的常规方法。 In the present invention, unless otherwise specified, all parts and percentages are weight units, and all equipment and raw materials can be purchased from the market or commonly used in this industry. The methods in the following examples, unless otherwise specified, are conventional methods in the art.
实施例1:Example 1:
本实施例采用HDDR工艺制备的各向异性粘结NdFeB磁粉作为原料磁粉,其最大磁能积为(BH)max=288kJ/m3,内禀矫顽力Hcj=1040kA/m。 In this example, the anisotropic bonded NdFeB magnetic powder prepared by HDDR technology is used as the raw material magnetic powder, the maximum energy product of which is (BH)max=288kJ/m 3 , and the intrinsic coercive force Hcj=1040kA/m.
一种室温湿压成型各向异性粘结NdFeB磁体的制备方法,包括: A method for preparing an anisotropic bonded NdFeB magnet formed by wet pressing at room temperature, comprising:
原料配比:0.1wt%的硅烷偶联剂(市售KH550)、99.6wt%的各向异性粘结NdFeB磁粉、0.3wt%的环氧树脂粘结剂。 Raw material ratio: 0.1wt% silane coupling agent (commercially available KH550), 99.6wt% anisotropic bonded NdFeB magnetic powder, 0.3wt% epoxy resin binder.
(1)、磁粉表面改性工序:将0.1wt%的硅烷偶联剂(市售KH550)用乙醇溶解,然后加入99.6wt%的各向异性粘结NdFeB磁粉并混合均匀,然后在40~80℃下烘干,得到表面改性的各向异性粘结NdFeB磁粉。 (1) Surface modification process of magnetic powder: Dissolve 0.1wt% silane coupling agent (commercially available KH550) in ethanol, then add 99.6wt% anisotropic bonded NdFeB magnetic powder and mix evenly, then and drying at ℃ to obtain surface-modified anisotropic bonded NdFeB magnetic powder.
(2)、粘结剂与磁粉混合工序:将0.3wt%的环氧树脂粘结剂用丙酮溶解,加入上述经过表面改性的各向异性粘结NdFeB磁粉中,并混合均匀、烘干。 (2) Binder and magnetic powder mixing process: dissolve 0.3wt% epoxy resin binder with acetone, add to the surface-modified anisotropic bonded NdFeB magnetic powder, mix evenly, and dry.
(3)、磁粉浆料制备工序:将磁粉-环氧树脂混合物置于行星式球磨机中,加入十二烷基苯磺酸钠(磁粉质量的0.1%)、乙醇(磁粉质量的50%)以及硬脂酸钙(磁粉质量的0.1%),进行机械球磨,形成磁粉浆料,其中,磨球采用密度为3.97g/cm3氧化铝球。 (3) Preparation of magnetic powder slurry: Put the magnetic powder-epoxy resin mixture in a planetary ball mill, add sodium dodecylbenzenesulfonate (0.1% of the mass of the magnetic powder), ethanol (50% of the mass of the magnetic powder) and Calcium stearate (0.1% of the mass of the magnetic powder) is mechanically ball milled to form a magnetic powder slurry, wherein the grinding balls are alumina balls with a density of 3.97g/cm 3 .
(4)、磁场模压成型工序:将磁粉浆料注入模具中,室温下压制成Φ10mm×10mm的磁体标样,压制磁场1.5T,压制压力9t/cm2。 (4) Magnetic field compression molding process: inject the magnetic powder slurry into the mold, and press at room temperature to form a Φ10mm×10mm magnet standard sample, with a pressing magnetic field of 1.5T and a pressing pressure of 9t/cm 2 .
(5)、真空固化工序:将磁体标样在140℃下真空固化3h。 (5) Vacuum curing process: The magnet standard sample is vacuum cured at 140° C. for 3 hours.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到172kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 172kJ/m 3 .
实施例2Example 2
本实施例其他操作同实施例1,不同之处在于:所采用的磁场为1T。 Other operations of this embodiment are the same as those of Embodiment 1, except that the magnetic field used is 1T.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到155.6kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH) max reached 155.6 kJ/m 3 .
实施例3Example 3
本实施例其他操作同实施例1,不同之处在于:所采用的磁场为2T。 Other operations of this embodiment are the same as those of Embodiment 1, except that the magnetic field used is 2T.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到173.6kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH) max reached 173.6 kJ/m 3 .
实施例4Example 4
本实施例其他操作同实施例1,不同之处在于:所采用的压制压力为3t/cm2。 Other operations of this embodiment are the same as those of Embodiment 1, except that the pressing pressure used is 3t/cm 2 .
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到91kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 91kJ/m 3 .
实施例5Example 5
本实施例其他操作同实施例1,不同之处在于:所采用的压制压力为5t/cm2。 Other operations of this embodiment are the same as those of Embodiment 1, except that the pressing pressure used is 5 t/cm 2 .
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到133.6kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH) max reached 133.6 kJ/m 3 .
实施例6Example 6
本实施例其他操作同实施例1,不同之处在于:所采用的压制压力为9t/cm2。 Other operations of this embodiment are the same as those of Embodiment 1, except that the pressing pressure used is 9t/cm 2 .
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到142kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 142kJ/m 3 .
实施例7Example 7
本实施例其他操作同实施例1,不同之处在于:十二烷基苯磺酸钠的用量为磁粉质量的1%。 Other operations of this embodiment are the same as those of Embodiment 1, except that the amount of sodium dodecylbenzenesulfonate is 1% of the mass of the magnetic powder.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到154kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 154kJ/m 3 .
实施例8Example 8
本实施例其他操作同实施例1,不同之处在于:硬脂酸钙用量为磁粉质量的1%。 Other operations of this embodiment are the same as those of Embodiment 1, except that the amount of calcium stearate is 1% of the mass of the magnetic powder.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到165kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 165kJ/m 3 .
比较例1Comparative example 1
本实施例其他操作同实施例1,不同之处在于:未进行机械球磨工序。 Other operations of this embodiment are the same as those of Embodiment 1, except that no mechanical ball milling process is performed.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到112.3kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 112.3kJ/m 3 .
比较例2Comparative example 2
本实施例其他操作同实施例1,不同之处在于:所采用磨球为密度为7.5 g/cm3不锈钢球。 Other operations of this embodiment are the same as those in Embodiment 1, except that the grinding balls used are stainless steel balls with a density of 7.5 g/cm 3 .
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到150.2kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH)max reached 150.2kJ/m 3 .
比较例3Comparative example 3
本实施例其他操作同实施例1,不同之处在于:未加入表面活性剂。 Other operations of this embodiment are the same as those of Embodiment 1, except that no surfactant is added.
将本实施例得到的磁体标样进行检测,磁能积(BH)max达到132.6kJ/m3。 The magnet standard sample obtained in this embodiment was tested, and the magnetic energy product (BH) max reached 132.6 kJ/m 3 .
比较例4Comparative example 4
本比较例采用的各向异性磁粉同实施例1,工艺步骤如下: The anisotropic magnetic powder that this comparative example adopts is the same as embodiment 1, and the processing steps are as follows:
1、将0.1wt%的偶联剂用乙醇溶解,然后加入99.6wt%的各向异性粘结NdFeB磁粉并混合均匀,然后在40~80℃下烘干,得到表面改性的各向异性粘结NdFeB磁粉。 1. Dissolve 0.1wt% coupling agent in ethanol, then add 99.6wt% anisotropic bonding NdFeB magnetic powder and mix evenly, then dry at 40-80°C to obtain surface-modified anisotropic bonding Junction NdFeB magnetic powder.
2、将0.3wt%的环氧树脂粘结剂用丙酮溶解,加入上述经过表面改性的各向异性粘结NdFeB磁粉中,并混合均匀、烘干。 2. Dissolve 0.3wt% epoxy resin binder with acetone, add to the surface-modified anisotropic bonded NdFeB magnetic powder, mix evenly, and dry.
3、将粘结剂放入模具中,室温下磁场干压成型,磁场1.5T,压力9t/cm2。 3. Put the binder into the mold, and perform dry pressing in a magnetic field at room temperature, with a magnetic field of 1.5T and a pressure of 9t/cm 2 .
4、将磁体标样在140℃下真空固化3h。 4. Vacuum solidify the magnet standard sample at 140°C for 3 hours.
将本比较例得到的磁体标样进行检测,磁能积(BH)max为78kJ/m3。 The magnet standard sample obtained in this comparative example was tested, and the magnetic energy product (BH)max was 78kJ/m 3 .
比较例5Comparative Example 5
本比较例其他操作同比较例4,不同之处在于:成型为温压成型,成型温度为130℃。 Other operations of this comparative example are the same as those of Comparative Example 4, except that the forming is warm pressing and the forming temperature is 130°C.
将本比较例得到的磁体标样进行检测,磁能积(BH)max为178kJ/m3,磁性能略高于室温湿压成型的各向异性粘结NdFeB磁体,但是生产工艺复杂,且生产效率低。 The magnet standard sample obtained in this comparative example is tested, and the magnetic energy product (BH)max is 178kJ/m 3 , and the magnetic performance is slightly higher than that of the anisotropic bonded NdFeB magnet formed by wet pressing at room temperature, but the production process is complicated and the production efficiency is low. Low.
上述优选实施例只是用于说明和解释本发明的内容,并不构成对本发明内容的限制。尽管发明人已经对本发明做了较为详细地列举,但是,本领域的技术人员根据发明内容部分和实施例所揭示的内容,能对所描述的具体实施例做各种各样的修改或/和补充或采用类似的方式来替代是显然的,并能实现本发明的技术效果,因此,此处不再一一赘述。本发明中出现的术语用于对本发明技术方案的阐述和理解,并不构成对本发明的限制。 The above preferred embodiments are only used to illustrate and explain the content of the present invention, and do not constitute a limitation to the content of the present invention. Although the inventor has listed the present invention in detail, those skilled in the art can make various modifications or/and Supplementation or substitution in a similar manner is obvious and can achieve the technical effect of the present invention, so details will not be repeated here. The terms appearing in the present invention are used to explain and understand the technical solutions of the present invention, and do not constitute limitations to the present invention.
Claims (4)