CN102554183B - Method for low-pressure casting of aluminium alloy patterned ring by using low-pressure casting mould - Google Patents
Method for low-pressure casting of aluminium alloy patterned ring by using low-pressure casting mould Download PDFInfo
- Publication number
- CN102554183B CN102554183B CN 201210016080 CN201210016080A CN102554183B CN 102554183 B CN102554183 B CN 102554183B CN 201210016080 CN201210016080 CN 201210016080 CN 201210016080 A CN201210016080 A CN 201210016080A CN 102554183 B CN102554183 B CN 102554183B
- Authority
- CN
- China
- Prior art keywords
- liquid flowing
- pressure casting
- cooling liquid
- external mold
- low pressure
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
The invention discloses a method for low-pressure casting of an aluminium alloy patterned ring by using a low-pressure casting mould. The method is conducted by the following steps of: A, sequentially pre-heating an outer mould, a plaster mould core and a pouring gate to the temperatures of 350 DEG C, 110 DEG C and 400 DEG C, respectively; B, mould filling process, that is, pouring aluminium liquid into a mould cavity from the pouring gate with the pouring temperature being 700 DEG C, filling pressure being 0.3bar and filling speed being 0.007bar/s, maintaining the pressure at 1.0bar for 2000seconds within 50-60 seconds after mould filling; C, filling cooling water into a cooling liquid runner of the outer mould from a water inlet while maintaining the pressure, enabling the cooling water to flow out of a water outlet after going around the outer mold in the runner for a circle, wherein the flow of the cooling water is 150-200cm<3>/s and the time of duration is 500-600 seconds; and D, promoting a casting piece to cool to the temperature of 550 DEG C within 300 seconds by the cooling water taking away heat, and pressure relief and demould are conducted when the temperature of the casting piece is cooled to the temperature of 350 DEG C.
Description
Technical field:
The present invention relates to a kind of method that adopts the aluminum alloy pattern ring low pressure casting die to carry out low pressure casting.
Background technology:
Aluminum alloy pattern ring is the vitals that is used for sulfidization molding tyre tread in the tire-mold, the processing mode of these parts, at present both at home and abroad widespread usage mainly contain following three kinds:
1, artistic carving: be applicable to load-carrying loose tool tool;
2, galvano-cautery technology: be applicable to load-carrying tire and riding loose tool tool;
3, aluminum alloy casting technique: be applicable to riding loose tool tool.
For the requirement of security, comfortableness and aesthetic property, riding tire Pattern Design is than load-carrying tire complexity, and the form accuracy of decorative pattern and dimension precision requirement are very high.Therefore, the main aluminum alloy casting technique that adopts of the pattern ring of mould processing.
At present, the aluminum alloy pattern ring casting technique, general have two kinds of low pressure casting and gravitational castings.Wherein low pressure casting is with its advanced technology, and casting density height, the advantage that intensity is good become the leading trend of pattern ring casting technique day by day.But because of its complex process, equipment and technical parameter determine be difficult to hold, very big to the influence of product qualified rate.
In conjunction with Fig. 3, the cast principle of low pressure casting is: model is positioned at the top of crucible 1, aluminium liquid 2 passes through stalk 3, running channel 4 under certain pressure, rise in the die cavity 5, be full of pressurize a period of time behind the die cavity, make the crystallization under pressure of aluminium liquid, solidify, after meeting the requirements of chilling temperature, release, the demoulding.
The gypsum core rod 12 coaxial cavity centers interior and the gypsum core rod that are arranged at external mold 6 have heap sand 13, the outer wall of the inwall of external mold and gypsum core rod 12 forms the die cavity 5 of mould, be provided with plasterboard 14 in the sealing of the bottom of gypsum core rod, form the running channel 4 that is communicated with die cavity between plasterboard and the bed die 15
The running channel 4 of low pressure casting is below die cavity 5, and the feeding process is undertaken by running channel by pressure.Therefore foundry goods to solidify order should be from inside to outside, from top to bottom, feeding is carried out by running channel in the bottom of final set, the order of solidifying of foundry goods is: A → B → C → D → E → F, if can accomplish this point, the surface of foundry goods and internal soundness all can be guaranteed.
The bottom of external mold 6 has certain conical surface angle, and it act as: 1, guarantee foundry goods cooling order from top to bottom.2, guarantee the easy demoulding of foundry goods.
Because the particularity of mould structure, the wall thickness variation of pattern ring product is relatively large, and under the certain situation of same model outer profile size, internal diameter can have multiple variation according to tire specification.Make the scope of pattern ring wall thickness dimension not wait from 40-100mm.Therefore, the external mold of identical parameters and running channel are during the foundry goods of cast wall thickness more than 80mm, because aluminium liquid weight is many, thermal capacity is relatively large, cool time is long, causes the foundry goods condensation to occur in sequence variation, and running channel position F point is prior to the E point cooling of foundry goods, blocked the feeding passage, cause the E point feeding deficiency of foundry goods, produce pore and shrinkage defect, cause when serious and scrap.
In view of this, when the bigger pattern ring product of cast wall thickness dimension, there are a lot of technological deficiencies in existing cast outer mold structure and technological parameter, and its product percent of pass is difficult to guarantee that this is the technical barrier that we are badly in need of solving.
Summary of the invention:
For overcoming the defective of prior art, the object of the present invention is to provide a kind of method that adopts the aluminum alloy pattern ring low pressure casting die to carry out low pressure casting, make foundry goods can accelerate local cooling velocity on request, the condensation of realizing ideal order.
Technical solution problem of the present invention adopts following technical scheme:
A kind of method that adopts the aluminum alloy pattern ring low pressure casting die to carry out low pressure casting, described mould comprises external mold, gypsum core rod and bed die, described external mold is its inside of truncated cone-shaped generally and is cavity, the coaxial cavity center interior and the gypsum core rod that is arranged at external mold of described gypsum core rod has heap sand, the outer wall of the inwall of described external mold and described gypsum core rod forms the die cavity of mould, be provided with plasterboard in the sealing of the bottom of gypsum core rod, form the running channel that is communicated with described die cavity between described plasterboard and the described bed die, described external mold comprises that the inside that is truncated cone-shaped generally is the outer mould body of cavity, outside described, be provided with cooling liquid flowing channel near its place, bottom in the mould body, described cooling liquid flowing channel circumferential hoop is one week of mould body outside described, and in cooling liquid flowing channel, be provided with dividing plate, be respectively arranged with water inlet tap and the faucet of cooling liquid flowing channel in the both sides of described dividing plate;
Described method is carried out successively by following operation:
A, determine casting technological parameter: external mold is preheated to 350 ℃, 110 ℃ of gypsum core rod preheatings, and running channel is preheated to 400 ℃;
B, cavity filling process, namely by running channel cast aluminum liquid in the die cavity, pouring temperature is 700 ℃; Mold filling pressure is 0.3bar, and filling velocity is 0.007bar/s, carries out pressurize after aluminium liquid is full of model in the 50-60s, and dwell pressure maintains 1.0bar, and the dwell time is 2000s;
C, in pressurize, in the cooling liquid flowing channel of external mold, charge into cooling water by water inlet tap, cooling water flows out from faucet around the external mold back of rounding in runner, the flow of cooling water is 150-200cm
3/ s, duration 500-600s;
D, cooling water are taken away heat and are impelled foundry goods to be cooled to 550 ℃ in 300s, when casting temperature is cooled to 350 ℃, can carry out release, the demoulding, and foundry goods continues cooling at room temperature after the demoulding, and casting process is finished.
Design feature of the present invention also is:
The difference in height of the center of described cooling liquid flowing channel and described outer mould body bottom surface is 1/4 of whole external mold body height.
The arranged outside of described cooling liquid flowing channel has shrouding that described cooling liquid flowing channel is formed sealing, and the outer wall of described shrouding and the outer wall of described outer mould body are in same plane.
The cross-sectional area of described cooling liquid flowing channel is 15cm
2, the wall thickness of the outer mould body of cooling liquid flowing channel inboard is 15mm.
Described water inlet tap is 1/2, and " pipe, described faucet is 3/4 " is managed, and is provided with flowmeter and switch valve in the connecting line of water inlet tap and outside water supply line.
Basic principle of the present invention:
As stated in the Background Art, in the process of low pressure casting, the condensation of foundry goods order should be from inside to outside, from top to bottom, needs when solidify the foundry goods bottom to carry out feeding by running channel.Therefore, the position is cooled off at the running channel place at last.For guaranteeing this order, in technological equipment external mold and one timing of running channel model, as thick-walled casting, just must consider to accelerate the cooling velocity problem of foundry goods bottom.
The present invention has designed novel cast outer mold structure, namely on original structure size basis, a cooling liquid flowing channel is set in the mould body outside, namely forms the circular passage that has nozzle and spout along the external mold circumferencial direction.Be provided with a dividing plate between the nozzle and spout, after the assurance cooling water rounds along the external mold circumferencial direction, discharge from faucet.
During the product cast, after die cavity is full of, charge into cooling water continuously to water inlet tap, circulation was discharged by faucet after one week.Because holding, specific heat of water is 4.2x10
3J/kg ℃ is 9 times of steel, when cooling water with 200cm
3When the flow of/s charged into continuously and discharges, the heat of taking away in initial 100s was 10 times that co-content steel external mold absorbs heat at ambient temperature.Therefore, can realize accelerating the purpose of foundry goods bottom cooling velocity, make temperature of aluminum liquid in 300s, can be dropped to 550 ℃ of solidus temperature by 700 ℃ of pouring temperature, reach desirable condensation sequence requirement.
Compared with the prior art, beneficial effect of the present invention is embodied in:
1, is provided with cooling liquid flowing channel in the outer mould body of mould of the present invention, by the cooling water around external mold the bottom of foundry goods is cooled off prior to running channel, not only can shorten and fill type insulation, dwell time, reduce to 2000s by original 3300s, save electric power, improve work efficiency.What is more important has guaranteed the reasonable realization of super large wall thickness foundry goods cooling order, makes the foundry goods bottom be able to abundant feeding.Solve original mould and easily made foundry goods produce shrinkage porosite, gas hole defect problem, avoided product to scrap because casting flaw causes.
2, original mould and pouring technology thereof because foundry goods is long cool time, cause the shrinkage factor at upper and lower bore place to differ bigger, and top is 0.013, and the bottom is 0.014.After mould of the present invention had been realized the quick cooling of foundry goods bottom heavy wall, the shrinkage coefficient of upper and lower bore was very nearly the same, is 0.013, brought convenience for the accurate formulation of casting technological parameter, had finally guaranteed the dimensional accuracy of foundry goods.
Description of drawings:
Fig. 1 is cavity filling process pressue-graph of the present invention; Fig. 2 is forced cooling method of the present invention and former method cooling curve comparison schematic diagram in the foundry goods cooling procedure, and A is former cooling curve among the figure, and B is cooling curve of the present invention; Fig. 3 is aluminum alloy pattern ring low pressure casting principle schematic; Fig. 4 is the partial structurtes schematic diagram of external mold of the present invention; Fig. 5 is that the A of Fig. 4 is to cross-sectional view.
Number in the figure: 1 crucible, 2 aluminium liquid, 3 stalks, 4 running channels, 5 die cavitys, 6 external molds, 7 cooling liquid flowing channels, 8 dividing plates, 9 water inlet taps, 10 faucets, 11 dividing plates, 12 gypsum core rods, 13 heap sands, 14 plasterboards, 15 bed dies.
Below pass through the specific embodiment, and the invention will be further described by reference to the accompanying drawings.
The specific embodiment:
Embodiment 1: with reference to Fig. 3-5, the external mold 6 of aluminum alloy pattern ring low pressure casting of the present invention, in its body, be provided with the cooling liquid flowing channel 7 of circumferential hoop around outer one week of mould body, the distance of its centre-to-centre spacing external mold bottom surface is 1/4 of external mold height, and in cooling liquid flowing channel, be provided with dividing plate 8, be respectively arranged with water inlet tap 9 and the faucet 10 of cooling liquid flowing channel in the both sides of dividing plate.
The arranged outside of cooling liquid flowing channel 7 has 11 pairs of described cooling liquid flowing channels of shrouding to form sealing, and the outer wall of shrouding 11 is in same plane with the outer wall of outer mould body.In specifically arranging, the cross-sectional area of cooling liquid flowing channel 7 is 15cm
2, the wall thickness of the outer mould body of its inboard is 15mm.Water inlet tap is 1/2, and " pipe, faucet is 3/4 " is managed, and is provided with flowmeter and switch valve in the connecting line of water inlet tap and outside water supply line.
Embodiment 2: in the present embodiment, casting technological parameter is pressed following condition enactment: 350 ℃ of external mold preheatings, 110 ℃ of gypsum core rod preheatings, 400 ℃ of running channel preheatings, 700 ℃ of pouring temperatures.Cavity filling process is undertaken by pressure curve shown in Figure 1, mold filling pressure 0.3bar, and filling velocity 0.007bar/s, pressurize 1.0bar, the time is 2000s.In this process, 50-60s after aluminium liquid is full of type, beginning charges into cooling water to external mold, control flow 150-200cm
3/ min continues to stop behind the 500-600s.After dwell time reaches 2000s, when casting temperature is down to 350 ℃, release, the demoulding, at room temperature continue cooling.The control of flow size is according to casting section thickness 80-100mm size, at 150-200cm
3Select in/s the scope, when the casting section thickness size was big, flow was got big value, otherwise gets the small value, and guaranteed that foundry goods is cooled to 550 ℃ in 300s, according to said method, can realize the quick cooling of foundry goods, obtained desirable condensation order.
Claims (4)
1. method that adopts the aluminum alloy pattern ring low pressure casting die to carry out low pressure casting, described mould comprises external mold, gypsum core rod and bed die, described external mold is its inside of truncated cone-shaped generally and is cavity, the coaxial cavity center interior and the gypsum core rod that is arranged at external mold of described gypsum core rod has heap sand, the outer wall of the inwall of described external mold and described gypsum core rod forms the die cavity of mould, be provided with plasterboard in the sealing of the bottom of gypsum core rod, form the running channel that is communicated with described die cavity between described plasterboard and the described bed die, described external mold comprises that the inside that is truncated cone-shaped generally is the outer mould body of cavity, outside described, be provided with cooling liquid flowing channel near its place, bottom in the mould body, described cooling liquid flowing channel circumferential hoop is one week of mould body outside described, and in cooling liquid flowing channel, be provided with dividing plate, be respectively arranged with water inlet tap and the faucet of cooling liquid flowing channel in the both sides of described dividing plate;
It is characterized in that described method carries out successively by following operation:
A, determine casting technological parameter: external mold is preheated to 350 ℃, 110 ℃ of gypsum core rod preheatings, and running channel is preheated to 400 ℃;
B, cavity filling process, namely by running channel cast aluminum liquid in the die cavity, pouring temperature is 700 ℃; Mold filling pressure is 0.3bar, and filling velocity is 0.007bar/s, carries out pressurize after aluminium liquid is full of model in the 50-60s, and dwell pressure maintains 1.0bar, and the dwell time is 2000s;
C, in pressurize, in the cooling liquid flowing channel of external mold, charge into cooling water by water inlet tap, cooling water flows out from faucet around the outer mould body back of rounding in runner, the flow of cooling water is 150-200cm
3/ s, duration 500-600s;
D, cooling water are taken away heat and are impelled foundry goods to be cooled to 550 ℃ in 300s, when casting temperature is cooled to 350 ℃, can carry out release, the demoulding, and foundry goods continues cooling at room temperature after the demoulding, and casting process is finished.
2. employing aluminum alloy pattern ring low pressure casting die according to claim 1 carries out the method for low pressure casting, it is characterized in that, the difference in height of the center of described cooling liquid flowing channel and described outer mould body bottom surface is 1/4 of whole external mold body height.
3. employing aluminum alloy pattern ring low pressure casting die according to claim 1 carries out the method for low pressure casting, it is characterized in that, the arranged outside of described cooling liquid flowing channel has shrouding that described cooling liquid flowing channel is formed sealing, and the outer wall of described shrouding and the outer wall of described outer mould body are in same plane.
4. employing aluminum alloy pattern ring low pressure casting die according to claim 2 carries out the method for low pressure casting, it is characterized in that, the cross-sectional area of described cooling liquid flowing channel is 15 cm
2, the wall thickness of the outer mould body of cooling liquid flowing channel inboard is 15mm.