CN102490236B - Production process method for wooden door - Google Patents

Production process method for wooden door Download PDF

Info

Publication number
CN102490236B
CN102490236B CN201110397668.0A CN201110397668A CN102490236B CN 102490236 B CN102490236 B CN 102490236B CN 201110397668 A CN201110397668 A CN 201110397668A CN 102490236 B CN102490236 B CN 102490236B
Authority
CN
China
Prior art keywords
door
step
workpiece
production process
process method
Prior art date
Application number
CN201110397668.0A
Other languages
Chinese (zh)
Other versions
CN102490236A (en
Inventor
王永宏
Original Assignee
北京市全富木制品有限公司
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 北京市全富木制品有限公司 filed Critical 北京市全富木制品有限公司
Priority to CN201110397668.0A priority Critical patent/CN102490236B/en
Publication of CN102490236A publication Critical patent/CN102490236A/en
Application granted granted Critical
Publication of CN102490236B publication Critical patent/CN102490236B/en

Abstract

The invention relates to a production process method for a wooden door and belongs to the technical field of building materials. The production process method comprises the following steps of: blanking; forming a frame; performing hot pressing; performing cold pressing; edging and precisely cutting; milling a door core board; manually sticking skin; punching a lock hole and hinge holes; performing trial assembly; and painting. The production process method has the advantages that: repeated steps are simplified; and the production efficiency is greatly improved.

Description

A kind of production process method for wooden door

Technical field

The present invention relates to a kind of production process method for wooden door, belong to building material technical field.

Background technology

Existing timber production technology is comparatively loaded down with trivial details, cannot enhance productivity.

Summary of the invention

In order to overcome the deficiency of prior art structure, the invention provides a kind of production process method for wooden door.

The technical solution adopted for the present invention to solve the technical problems is: comprise following steps:

Step 1: blanking.During thick sanction, length and width respectively strengthen 10mm.

Step 2: group frame.Corner is upright, and length and width respectively strengthen 10mm, central filler Shao Er Lante hollow particieboard, and lock wood, and after skeleton does anti-deformation process, upper press flattens.

Step 3: hot pressing.Before putting the workpiece needing hot pressing, heating platen and workpiece are cleaned out at every turn, confirm without any impurity, reserve hot pressing temperature and pressure, workpiece is slowly put into; The workpiece arrangement of putting into is orderly, each position uniform force; All positions are piled in each hot pressing as far as possible, and ensure that the thickness of every laminate material is identical with the facing material of every layer, facing material can not repeat; For preventing glue from doing, each material loading should complete in two minutes, when determining errorless and safe, then machined.

Step 4: cold pressing.The time of colding pressing should determine according to temperature, ensures curable adhesive layer, and gummed firmly; After pressurization, surface of the work is smooth, and bright and clean, hand touches no concave-convex, granular sensation.

Step 5: edging essence is cut out.Before putting into workpiece, pressing plate and workpiece are cleaned out; The workpiece put into prevents dislocation, aligns up and down, prevent from collapsing slag with central layer; Door leaf both sides tilt 2 degree, and all the other are all sawn into straight flange, prevent scuffing from touching scarce.

Step 6: milling door panel.During milling door panel, walk material firmly evenly, prevent from collapsing slag; Milling in proportion, size is accurate, prevents from collapsing slag.

Step 7: manual lagging.During with white glue with vinyl lagging, brush second time again after first pass drying, then press with flatiron; Slat plank shovel pressure.

Step 8: beat lockhole and hinge hole.With particular manufacturing craft, can hole after clamp.

Step 9: trial assembly.Door leaf and door pocket fit tightly.

Step 10: paint.Openpore need polish smooth, hole for nailing, gap need be tamped.

As combined blanking, indicating wooden skin material, indicating which kind of gate combination.

Housing width specifications is 800-2000mm, and dash board is 6mm medium-density plate; Lock box replaces lock wood.

If need hot pressing workpiece not pile, the backing plate for subsequent use of application workpiece uniform thickness is filled; Surface of the work after pressurization is smooth, seep through, lamination are basically identical from core, scuffing, impression, collision block, dislocation, greasy dirt, color.

Cut out material error when edging essence is cut out and be no more than 0.2mm.

Door panel needs the smooth in appearance of milling, smoother.

Phenomenons such as after Virgin's milk sticker is complete, gap must not be had, come unstuck, bubbling, wooden skin burst.

Note the opening direction of door when beating lockhole, hinge hole, note the upper and lower side of door, must not turn around, must not have and collapse slag, scuffing.

It is tight that door ornamental thread connects angle, must not gap; Need smooth between door leaf and door pocket, must not gap, door leaf must not have gap to rock.

Before polishing, need check openpore, for coming unstuck, bubbling, scratch, touch scarce product and do not process.

Benefit of the present invention is: the step simplifying repetition, and production efficiency is improved greatly.

Detailed description of the invention

Embodiment 1: step 1: blanking.During thick sanction, length and width respectively strengthen 10mm.

Step 2: group frame.Corner is upright, and length and width respectively strengthen 10mm, central filler Shao Er Lante hollow particieboard, and lock wood, and after skeleton does anti-deformation process, upper press flattens.

Step 3: hot pressing.Before putting the workpiece needing hot pressing, heating platen and workpiece are cleaned out at every turn, confirm without any impurity, reserve hot pressing temperature and pressure, workpiece is slowly put into; The workpiece arrangement of putting into is orderly, each position uniform force; All positions are piled in each hot pressing as far as possible, and ensure that the thickness of every laminate material is identical with the facing material of every layer, facing material can not repeat; For preventing glue from doing, each material loading should complete in two minutes, when determining errorless and safe, then machined.

Step 4: cold pressing.The time of colding pressing should determine according to temperature, ensures curable adhesive layer, and gummed firmly; After pressurization, surface of the work is smooth, and bright and clean, hand touches no concave-convex, granular sensation.

Step 5: edging essence is cut out.Before putting into workpiece, pressing plate and workpiece are cleaned out; The workpiece put into prevents dislocation, aligns up and down, prevent from collapsing slag with central layer; Door leaf both sides tilt 2 degree, and all the other are all sawn into straight flange, prevent scuffing from touching scarce.

Step 6: milling door panel.During milling door panel, walk material firmly evenly, prevent from collapsing slag; Milling in proportion, size is accurate, prevents from collapsing slag.

Step 7: manual lagging.During with white glue with vinyl lagging, brush second time again after first pass drying, then press with flatiron; Slat plank shovel pressure.

Step 8: beat lockhole and hinge hole.With particular manufacturing craft, can hole after clamp.

Step 9: trial assembly.Door leaf and door pocket fit tightly.

Step 10: paint.Openpore need polish smooth, hole for nailing, gap need be tamped.

Which kind of gate combination is embodiment 2: as combination blanking, indicate wooden skin material, indicate.

Embodiment 3: housing width specifications is 800-2000mm, dash board is 6mm medium-density plate; Lock box replaces lock wood.

Embodiment 4: if need hot pressing workpiece not pile, the backing plate for subsequent use of application workpiece uniform thickness is filled; Surface of the work after pressurization is smooth, seep through, lamination are basically identical from core, scuffing, impression, collision block, dislocation, greasy dirt, color.

Embodiment 5: cut out material error when edging essence is cut out and be no more than 0.2mm.

Embodiment 6: door panel needs the smooth in appearance of milling, smoother.

Embodiment 7: after Virgin's milk sticker is complete, phenomenons such as gap must not being had, come unstuck, bubbling, wooden skin burst.

Embodiment 8: the opening direction noting door when beating lockhole, hinge hole, notes the upper and lower side of door, must not turn around, must not have and collapse slag, scuffing.

Embodiment 9: it is tight that door ornamental thread connects angle, must not gap; Need smooth between door leaf and door pocket, must not gap, door leaf must not have gap to rock.

Embodiment 10: before polishing, need check openpore, for coming unstuck, bubbling, scratches, touches scarce product and do not process.

Claims (7)

1. a production process method for wooden door, is characterized in that, comprises following steps:
Step 1: blanking; During thick sanction, length and width respectively strengthen 10mm;
Step 2: group frame; Corner is upright, and length and width respectively strengthen 10mm, central filler Shao Er Lante hollow particieboard, and lock wood, and after skeleton does anti-deformation process, upper press flattens;
Step 3: hot pressing; Before putting the workpiece needing hot pressing, heating platen and workpiece are cleaned out at every turn, confirm without any impurity, reserve hot pressing temperature and pressure, workpiece is slowly put into; The workpiece arrangement of putting into is orderly, each position uniform force; All positions are piled in each hot pressing as far as possible, and ensure that the thickness of every laminate material is identical with the facing material of every layer, facing material can not repeat; For preventing glue from doing, each material loading should complete in two minutes, when determining errorless and safe, then machined;
Step 4: cold pressing; The time of colding pressing should determine according to temperature, ensures curable adhesive layer, and gummed firmly; After pressurization, surface of the work is smooth, and bright and clean, hand touches no concave-convex, granular sensation;
Step 5: edging essence is cut out; Before putting into workpiece, pressing plate and workpiece are cleaned out; The workpiece put into prevents dislocation, aligns up and down, prevent from collapsing slag with central layer; Door leaf both sides tilt 2 degree, and all the other are all sawn into straight flange, prevent scuffing from touching scarce;
Step 6: milling door panel; During milling door panel, walk material firmly evenly, prevent from collapsing slag; Milling in proportion, size is accurate, prevents from collapsing slag;
Step 7: manual lagging; During with white glue with vinyl lagging, brush second time again after first pass drying, then press with flatiron; Slat plank shovel pressure;
Step 8: beat lockhole and hinge hole; With particular manufacturing craft, can hole after clamp;
Step 9: trial assembly; Door leaf and door pocket fit tightly;
Step 10: paint; Openpore need polish smooth, hole for nailing, gap need be tamped;
Before polishing, need check openpore, for coming unstuck, bubbling, scratch, touch scarce product and do not process;
Housing width specifications is 800-2000mm, and dash board is 6mm medium-density plate; Lock box replaces lock wood;
Note the opening direction of door when beating lockhole, hinge hole, note the upper and lower side of door, must not turn around, must not have and collapse slag, scuffing.
2. a kind of production process method for wooden door according to claim 1, is characterized in that: combination blanking, indicates wooden skin material, indicates which kind of gate combination.
3. a kind of production process method for wooden door according to claim 1, is characterized in that: if need hot pressing workpiece not pile, and the backing plate for subsequent use of application workpiece uniform thickness is filled; Surface of the work after pressurization is smooth, seep through, lamination are basically identical from core, scuffing, impression, collision block, dislocation, greasy dirt, color.
4. a kind of production process method for wooden door according to claim 1, is characterized in that: cut out material error when edging essence is cut out and be no more than 0.2mm.
5. a kind of production process method for wooden door according to claim 1, is characterized in that: door panel needs the smooth in appearance of milling, smoother.
6. a kind of production process method for wooden door according to claim 1, is characterized in that: after Virgin's milk sticker is complete, must not have gap, come unstuck, bubbling, wooden skin burst phenomenon.
7. a kind of production process method for wooden door according to claim 1, is characterized in that: it is tight that door ornamental thread connects angle, must not gap; Need smooth between door leaf and door pocket, must not gap, door leaf must not have gap to rock.
CN201110397668.0A 2011-12-02 2011-12-02 Production process method for wooden door CN102490236B (en)