CN102358100B - Processing and manufacturing method for lacquer paintings of relief bare wood - Google Patents

Processing and manufacturing method for lacquer paintings of relief bare wood Download PDF

Info

Publication number
CN102358100B
CN102358100B CN 201110240636 CN201110240636A CN102358100B CN 102358100 B CN102358100 B CN 102358100B CN 201110240636 CN201110240636 CN 201110240636 CN 201110240636 A CN201110240636 A CN 201110240636A CN 102358100 B CN102358100 B CN 102358100B
Authority
CN
China
Prior art keywords
polyester
paint
tire
painting
embossment
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 201110240636
Other languages
Chinese (zh)
Other versions
CN102358100A (en
Inventor
李志国
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 201110240636 priority Critical patent/CN102358100B/en
Publication of CN102358100A publication Critical patent/CN102358100A/en
Application granted granted Critical
Publication of CN102358100B publication Critical patent/CN102358100B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to a processing and manufacturing method for lacquer paintings of relief bare wood, which comprises procedures including bare wood manufacturing, painting, carving, grinding, primer painting, pattern drawing through polyester color paints, finish painting, frame installing and assembling and the like. The pattern drawing through polyester color painting includes steps of blending the polyester color painting through polyester painting, polyester color concentrates and diluents, dipping the diluents color painting through a pointless flat writing brush and drawing the colored patterns on pattern outlines of the relief bare wood. Be organically combining wood relief technique and a polyester lacquer painting technique, brand-new art works which can vividly display artistic effects of animal furs, bird feathers, plant texture and grass sprouts and the like are manufactured, and the art works are three-dimensional, clear in images and vivid and forms an artistic expression form and artistic expression effect.

Description

A kind of processing and fabricating method of embossment wood tire lacquer painting
Technical field
The present invention relates to a kind of art drawing, specifically a kind of processing and fabricating method of embossment wood tire lacquer painting.
Background technology
At present, the popular wooden anaglyphy product of China are a lot, and the lacquer painting product is also a lot, and still, the problem complete of the same colour of wooden relief sculpture products is more serious, and the very difficult method with carving such as the skin texture of some thing shapes, texture shows; And lacquer painting mainly is to draw a picture with lacquer, and its works also have certain limitation, just is difficult to vivo show such as the fur of animal, subtleties such as trees flowers and plants in the scenery with hills and waters.
Summary of the invention
Purpose of the present invention just provides the processing and fabricating method of a kind of embossment wood tire lacquer painting, can not truly vivo show the problems such as the skin texture of the thing shapes such as animals and plants and texture to solve embossment and lacquer painting works.
The present invention is achieved in that
A kind of processing and fabricating method of embossment wood tire lacquer painting, carry out according to the following steps:
A, with the plank of drying by bonding, saw is neat, planing etc., is processed into wooden tire;
B, drawn rough sketch is replicated on the described wooden tire with modes such as copy papers, forms plate face pattern;
C, the described plate face pattern on the wooden tire is carved, formed embossment wood tire;
D, the convex-concave surface on the described embossment wood tire is carried out grinding process, make it smooth;
E, blend transparent polyester priming paint in the usual way, the transparent polyester priming paint that will convert with spray gun evenly is sprayed at the surface of described embossment wood tire, namely forms prime coat after spraying 2-3 times; After the prime coat drying, the flaw places such as the lip-deep pinhole of described embossment wood tire, crack are filled up and repair process; After prime coat is polished smooth, evenly spray again transparent polyester priming paint 2-3 times;
F, blend the polyester colored paint with Polyester Paint, polyester look essence and diluent, the tack writing brush that spends point dips described polyester colored paint, delineates colored pattern at the pattern contour of described embossment wood tire, and dries;
G, blend the transparent polyester finish paint in the usual way, to the surface of delineating the embossment wood tire works behind the colored pattern with spray gun with the evenly spraying 4-6 times of transparent polyester finish paint, form the protection surface layer;
Embossment wood tire lacquer painting finished product is made in h, upper ledge assembling.
Described polyester colored paint is to be mixed by Polyester Paint, polyester look essence and diluent to form, and its mixed ratio is: Ju Zhi Qi ︰ polyester Se Jing ︰ diluent=(0.1-0.2) ︰, 5 ︰ 10.Here, the addition of Polyester Paint is less, mainly is the toughness of utilizing it; Color is mainly derived from the polyester look smart; Diluent is used for adjusting viscosity, to utilize pen.Polyester Paint generally is to select water white paint vehicle, also can select approach or with the polyester look single-minded color that causes.Certainly, be the needs of pattern picture, can be first allot required color with the accurate adjustment of several polyester look, and then be mixed with Polyester Paint and diluent and become the polyester of required color colored paint.
The described tack writing brush that removes point is that the high-quality green tea section at common writing brush cuts off 4-6mm.High-quality green tea section cuts very little, and the front end of writing brush is difficult for scattering when delineating, and also just is not easy to draw out train of thought and coats with lacquer clearly line; It is too many that high-quality green tea section cuts, and pen head part has just lost corresponding elasticity, the flexible reduction of writing brush when delineating, and it is mellow and full and the lacquer line of certain dynamics arranged also just to be difficult for forming lines.
The present invention is by organically combining a kind of brand-new artistic expression of formation with wooden embossment and lacquer painting.And wherein distinctive polyester colored paint is delineated painted processing step, especially an outstanding feature of the present invention.One of characteristic of Polyester Paint is exactly that viscosity is large, can not brush evenly, because of this characteristic Polyester Paint is not used always in lacquer painting.The present invention through prolonged and repeated grope and put into practice after find, utilize the above-mentioned characteristic of Polyester Paint, the drawing tool that cooperates the transformation of the way, can draw out clearly coloured line segment at embossment wood tire on the contrary, and this clearly coloured line segment can be vivid on the picture of embossment wood tire, vivo show animal skin, poultry feather, the skin texture of the multiple thing shapes such as plant texture and little blade of grass seedling, texture and other precise and tiny details parts, the third dimension of made artistic work is strong, image definition, life-like, and these display forms can't show on original wooden embossment works or lacquer painting works at all.Therefore, the present invention is by the combination of wooden embossment skill and technique and polyester lacquer painting skill and technique, produce a kind of brand-new artistic work that can vivid, vivo show the artistic effects such as animal skin, poultry feather, plant texture and little blade of grass seedling, formed a kind of artistic expression and artistic representing effect that is different from existing wooden embossment works and lacquer painting works.
The specific embodiment
The processing and fabricating method of embossment wood tire lacquer painting of the present invention is to carry out according to the following steps:
1, makes wooden tire: the plank that drying is handled well (is generally selected cork, such as linden etc.) be sawn into required length (will reserve allowance), behind torn edges, emission rate, tight seam, with binding agents such as pig skin maw or air bladders, plank is bonding firmly, form a dull and stereotyped plate face that breadth is larger.After to be dried, by the redundance of required actual size saw trimming edge, plate face and edge are smooth, form the wooden tire of works.
2, draw: pre-rendered good rough sketch is replicated in carbon paper on the plate face of wooden tire, forms plate face pattern.Certainly also can adopt other modes such as inscription rubbing to copy rough sketch at wooden tire.
3, engraving: shovel at the end first (namely the recess in the plate face pattern being carved out first), shovel again protruding place, one by one each pattern is carved.In the shovel process at the end, can use small-sized engraving machine.Depiction is to finish with graver is manual.Graver comprises the engraving cutter of the multiple routines such as oblique blade cutter, round mouth cutter, angle cutter, graver, can select flexibly according to the needs of picture.
4, polishing: after all carving the pattern on the wooden tire well, namely form embossment wood tire, and then with 240 #Concavo-convex place on the waterproof abrasive paper dry grinding embossment wood tire picture is until polish smooth.
5, priming: blend transparent polyester priming paint by traditional usual manner, the transparent polyester priming paint that will convert with spray gun evenly is sprayed at the surface of embossment wood tire works, connect and spray 2-3 times, prime coat.Surface drying through 2-4 hours, make the prime coat drying after, with putty shovel transparent polyester putty is smeared in flaw places such as the embossment wood lip-deep pinhole of tire and cracks, fill up and repair process.After parching Deng transparent polyester putty, carry out again grinding process.The mode of polishing is: use first 240 #Waterproof abrasive paper dips in water polishing layer of paint, after polishing is level and smooth, and the remaining lacquer of polishing and with clear water flush away work surface, and then with 360 #The waterproof abrasive paper refinement polishes smooth.After polishing finishes, with spray gun the polyester transparent finish paint is sprayed at the surface of embossment wood tire works, connects and spray 2-3 times, make the surface of embossment wood tire reach smooth, smooth.
6, delineate pattern with the polyester colored paint: blend first the polyester colored paint, the color required according to picture, smart and diluent is mixed with a small amount of Polyester Paint and polyester look, and the mixed ratio general control exists: ︰ 5 ︰ 10 of Ju Zhi Qi ︰ polyester Se Jing ︰ diluent=(0.1-0.2); Be mixed behind the polyester colored paint of blending out various required colors, use again common writing brush, cut off the high-quality green tea part of 4-6mm, make the tack writing brush; Dip the polyester colored paint with the tack writing brush, adopt the brush of advancing side by side, the mode of delineating of smearing, putting forward, just can on embossment wood tire, delineate painted by the good pattern contour of engraving.Draw required color and concentration can be determined according to the color needs on the picture and thickness sense.
7, topcoating: blend in the usual way the transparent polyester finish paint, in clean paint spray booth, the transparent polyester finish paint that will convert with spray gun evenly is sprayed at the surface of delineating the embossment wood tire works behind the lacquer colored pattern.During spraying, note giving the lacquer amount and to tolerance, and getting hold of distance and the angle of spray gun and works of spray gun.Will work the embossment finished wood moulding bed keeping flat before the spray, the height that has added is advisable about with 50cm, so that paint spraying.Be spray from an end of embossment wood tire works during paint spraying, be sprayed onto the other end always, stop-spraying not can not connect stubble midway.After spray was good, it was dry to put into drying shed.
8, upper ledge assembling: frame for installing around the good embossment wood tire works of drying, and assembling fixes, and so just can be made into width of cloth embossment wood tire lacquer painting finished product.
In processing and fabricating method of the present invention, the gimmick of delineating with polyester colored paint performance animal wool is, with the tack writing brush that cuts off high-quality green tea, dip the polyester colored paint of converting in right amount, continuity point is smeared lightly on embossment wood tire picture, the hair of tack writing brush is in the state of scattering all the time, advances side by side, and such one can draw several hairs.During picture, hair root is first stroke of a Chinese character place, and high-quality green tea is for receiving the pen place, and will note the trend of animal wool, is also noted that the chiaroscuro effect etc. of length, color and the picture of different animals hair.
The gimmick of delineating gimmick and picture animal wool with polyester colored paint performance green grass is basic identical, notices that the first stroke of a Chinese character will be from the bottom up, and slightly radian has to from left to right.Note the relationship between light and dark on the picture---the where there is light look shallow, the few point of grass; The dark place color depth, careless multiple spot.Note careless height and density etc.
The gimmick of delineating gimmick and picture animal wool with polyester colored paint performance plant leaf and petal texture is similar, note trend and the density of plant leaf and petal texture, also is the root first stroke of a Chinese character from texture, receives pen in the tip of texture; Also to show chiaroscuro effect during picture.
Blending and spraying of polyester priming paint and polyester finish coat all is that furniture is made the routine techniques in the industry.Why the present invention will use polyester priming paint and polyester finish coat to spray the end, spray plane, will match with the polyester colored paint of delineating pattern exactly, in order to avoid react between the inhomogeneity paint.Using transparent polyester putty also is this reason.

Claims (2)

1. the processing and fabricating method of an embossment wood tire lacquer painting is characterized in that, carries out according to the following steps:
A, with the plank of drying by bonding, saw is neat, planing, makes wooden tire;
B, drawn rough sketch is replicated on the described wooden tire, forms plate face pattern;
C, the described plate face pattern on the wooden tire is carved, formed embossment wood tire;
D, the convex-concave surface on the described embossment wood tire is carried out grinding process;
E, blend transparent polyester priming paint, the transparent polyester priming paint that will convert with spray gun evenly is sprayed at the surface of described embossment wood tire, namely forms prime coat after spraying 2-3 times; After the prime coat drying, the lip-deep pinhole of described embossment wood tire, crack flaw place are filled up and repair process; After prime coat is polished smooth, evenly spray again transparent polyester priming paint 2-3 times;
F, blend the polyester colored paint with Polyester Paint, polyester look essence and diluent, the tack writing brush that spends point dips described polyester colored paint, delineates colored pattern at the pattern contour of described embossment wood tire, and dries; The described tack writing brush that removes point is that the high-quality green tea section at common writing brush cuts off 4-6mm;
G, blend the transparent polyester finish paint, to the surface of delineating the embossment wood tire works behind the lacquer colored pattern with spray gun with the evenly spraying 4-6 times of transparent polyester finish paint, form the protection surface layer;
Embossment wood tire lacquer painting finished product is made in h, upper ledge assembling.
2. the processing and fabricating method of embossment according to claim 1 wood tire lacquer painting, it is characterized in that, described polyester colored paint is to be mixed by Polyester Paint, polyester look essence and diluent to form, and its mixed ratio is: ︰ 5 ︰ 10 of Ju Zhi Qi ︰ polyester Se Jing ︰ diluent=(0.1-0.2).
CN 201110240636 2011-08-22 2011-08-22 Processing and manufacturing method for lacquer paintings of relief bare wood Expired - Fee Related CN102358100B (en)