CN101334119A CNA200710118131XA CN200710118131A CN101334119A CN 101334119 A CN101334119 A CN 101334119A CN A200710118131X A CNA200710118131X A CN A200710118131XA CN 200710118131 A CN200710118131 A CN 200710118131A CN 101334119 A CN101334119 A CN 101334119A
Authority
CN
China
Prior art keywords
pipe
welding
internal lining
nipple
metal composite
Prior art date
Application number
CNA200710118131XA
Other languages
Chinese (zh)
Other versions
CN100549486C (en
Inventor
李为卫
熊庆人
霍春勇
杨龙
严密林
Original Assignee
中国石油天然气集团公司
中国石油天然气集团公司管材研究所
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 中国石油天然气集团公司, 中国石油天然气集团公司管材研究所 filed Critical 中国石油天然气集团公司
Priority to CNB200710118131XA priority Critical patent/CN100549486C/en
Publication of CN101334119A publication Critical patent/CN101334119A/en
Application granted granted Critical
Publication of CN100549486C publication Critical patent/CN100549486C/en

Links

Abstract

The invention relates to a novel bimetallic composite pipe, which is applied in exploiting oil and natural gas fields. The novel bimetallic composite pipe is characterized in that an inner lining pipe is arranged in an outer wall pipe. Short joints are welded at both ends of the outer wall pipe, welding seams are arranged between the outer wall pipe and the short joints, and both end parts of the inner lining pipe are welded on the inner wall of the short joints. At least 1 through hole with the diameter of 2 to 10 millimeters is drilled on the wall of the outer wall pipe. Electric welding is adopted to completely weld the through hole after the water pressure test, namely, electric welding is used for solidly filling the through hole after the water pressure test. Screw threads are machined at both ends of the novel bimetallic composite pipe or the both ends of the novel bimetallic composite pipe are machined into two welding grooves. The novel bimetallic composite pipe has the advantages that a carbon steel pipe or a low alloy steel pipe is adopted as the substrate material of the outer wall pipe, to exert the superior capability of mechanics of machinery and the low price characteristic of the carbon steel pipe or the low alloy steel pipe; the inner lining adopting layer corrosion resistant alloy is provided with excellent corrosion resistant capability and superior capability of mechanics of machinery. The screw threads coupling connection sealing problem and the bimetallic composite pipe ground welding problem occurring when the prior bimetallic composite pipes are in use are thoroughly solved, the application field of the bimetallic composite pipe is enlarged, and the cost of the oil field exploitation is saved.

Description

Novel dual metal composite pipes and manufacture method
Technical field
The invention belongs to the steel tube fabrication technique field, relate to a kind of novel dual metal composite pipes structure and manufacturing technology thereof that is used for oil, gas field exploitation.
Background technique
Petroleum industry is the industry of widely applying tubing, needs a large amount of steel pipes in the oilfield exploitation procedure.In the oilfield exploitation procedure, inevitably run into and contain H 2S, CO 2, medium such as Cl, these media have very strong corrosivity to tubing.In oilfield exploitation procedure, corrosion is the serious problems that exist from start to finish, and it has not only caused enormous economic loss, and often brings some catastrophic effects, for example: casualties, stop work and production and environmental pollution etc.Corrosion is a lot of to the accident that petroleum industry causes, and annual economic loss is very big, therefore tubing has been proposed higher anti-corrosion requirement.The tubing of selecting function admirable for use is the major measure that prevents the corrosion accident.But, the corrosion resistance of the carbon steel or low alloy steel tubing that price general charged is cheap is relatively poor, and the price height of material such as the good stainless steel of corrosion resistance, nickel-base alloy, in order to save the consumption of the high material of price, people begin one's study, make and select for use composite pipe, comprise composite bimetal pipe.
Composite bimetal pipe is made up of the bushing pipe of outer field parent tube and internal layer.The at present domestic manufacture method that generally adopts is that machinery is fitted, as technological methodes such as hot extrusion, cold-drawn, cold spinnings.Owing to have the gap between parent tube and the bushing pipe, when local etching appears in bushing pipe, Korrosionsmedium infiltrates gap between parent tube and the bushing pipe, will form crevice corrosion, quickens corrosive pipeline.So, need new method and make composite bimetal pipe, replace adopting the composite pipe of existing mechanical applying method manufacturing.
The members such as pressurized container that adopt bi-metal composite panel to make are widely applied in various industry, good economic benefit and social benefit have been obtained, small-bore composite bimetal pipe material is used in industries such as automobile, Aeronautics and Astronautics, also begin to attempt adopting composite pipe in recent years in the oil-gas field development, in a plurality of oil field developments such as long celebrating, triumph, tooth Kazakhstan, use.
Comprising that common composite bimetal pipe is general is two-layer, and outer wall pipe matter is carbon steel or low alloy steel, and wall thickness is bigger, mainly bears external force or interior pressure, and interior pipe is generally stainless steel or nickel-base alloy, thickness less (below 4 millimeters).Composite bimetal pipe is fit to flange and connects.But the oil-gas field development down-hole generally adopts threaded collar joint to connect with tubing and casing, because the thinner thickness joint joint sealing difficulty of interior pipe is big, and poor reliability, medium can cause the pipe corrosion failure equally easily to external leakage.Under the condition of oil mining area field work, generally can only adopt welding method to connect aboveground composite bimetal pipe pipeline.Welding relates to the connection of dissimilar metal, difficult quality guarantee under the condition at the scene between the composite pipe.For this reason, composite bimetal pipe factory has also taked some measures, as turnup structure, end face soldering and sealing, pile mode such as limit in advance, reduces the difficulty of field welding, but these technology or thoroughly do not solve on-the-spot dissimilar steel Welding Problems, perhaps complex process.But the connection of composite bimetal pipe, the box cupling that comprises the down-hole pipe are threaded and being welded to connect of surface duct, and are insoluble problems.
Summary of the invention
The purpose of this invention is to provide a kind of novel dual metal composite pipes and manufacture method, production is fit to contain the composite bimetal pipe that uses in the oilfield exploitation procedure of Korrosionsmedium.Make composite bimetal pipe have better corrosion resistance and operational safety, the seal with screwed joint problem when solving the composite bimetal pipe use and the Welding Problems of surface duct, the cost of oil field development is saved in the use field of expansion composite bimetal pipe.
The structure of novel dual metal composite pipes of the present invention is:
Novel dual metal composite pipes of the present invention comprises outer wall pipe 1 and internal lining pipe 2, and it is characterized in that has internal lining pipe 2 in the outer wall pipe 1.The two ends of outer wall pipe 1 are welded with pipe nipple 4, between outer wall pipe 1 and the pipe nipple 4 weld seam are arranged, and the two end part of internal lining pipe 2 are welded on the inwall of pipe nipple 4.On outer wall pipe 1 wall, be drilled with the through hole 6 of at least one diameter at the 2-10 millimeter.The described through hole 6 that bores on outer wall pipe 1 wall is course of working holes, adopts electric welding to weld dead through hole 6 after the hydrostatic test, promptly mends through hole 6 real with electric welding after the hydrostatic test.The effect of through hole 6 has two: get rid of gap and residual gas between internal lining pipe 2 and the outer wall pipe 1 when utilizing the hydrostatic test, make outer wall pipe 1 and internal lining pipe 2 in conjunction with tightr; Check by the leakage situation of pipe in 6 pairs of the through holes during hydrostatic test.There is tubing round thread at the composite bimetal pipe two ends or is processed with the groove of welding usefulness.
The material of outer wall pipe 1 is a carbon steel or low alloy steel, and outer wall pipe 1 is mainly used in and bears external force or interior pressure during use.The internal diameter of outer wall pipe 1 is between the 60-500 millimeter, and the thickness of outer wall pipe 1 is between the 6-20 millimeter.The internal diameter of outer wall pipe 1 and thickness are determined according to the mechanical property of the actual employing of composite bimetal pipe material and flow, pressure and the stressing conditions etc. of composite bimetal pipe fed sheet of a media.Internal lining pipe 2 materials are stainless steel, nickel-base alloy or other corrosion resistant material, are mainly used in anticorrosive.Internal lining pipe 2 thickness are between the 1-4 millimeter.The material of pipe nipple 4 will have corrosion resistance, and will have sufficiently high intensity and good weldability material, as stainless steel, abros.
The manufacture method of novel dual metal composite pipes of the present invention is:
1., outer wall pipe 1, pipe nipple 4 and internal lining pipe 2 processing and fabricatings: outer wall pipe 1 endoporus is identical with pipe nipple 4 endoporus, and the external diameter difference of outer wall pipe 1 endoporus, pipe nipple 4 endoporus and internal lining pipe 2 is between the 1-3 millimeter.
2., clean the outer surface of outer wall pipe 1 endoporus and internal lining pipe 2, remove degreasing and oxide.
3., adopt welding methods such as melting, friction welding or instantaneous liquid-phase diffusion welding to carry out welding between outer wall pipe 1 and the pipe nipple 4, remove reinforcement or burrs inside and outside the weld seam 3, butt welded seam 3 is heat-treated in case of necessity.Type of heat treatment, method and parameter are more, decide according to concrete material, and this patent does not comprise this technology.
4., internal lining pipe 2 inserts in the outer wall pipe 1 and pipe nipple 4 that welds, and carries out compound.
5., the two ends with internal lining pipe 2 are welded on the inwall of pipe nipple 4 the two ends welding of pipe nipple 4 inwalls and internal lining pipe 2, formation seal angle weld seam;
6., pipe nipple 4 is sealed at both ends, carries out the hydrostatic test, the pressure of the hydrostatic test will be decided according to the strength grade of external diameter, thickness and the material of outer wall pipe, generally between 5-30MPa.Purpose is the bearing capacity of check novel dual metal composite pipes, and outer wall pipe 1 and internal lining pipe 2 are combined closely.Whether there is fluid seepage to go out by the 6 check internal lining pipes 2 of the through hole on the outer wall pipe 1;
7. as required, the novel dual metal composite pipes two ends are processed, as the novel dual metal composite pipes two ends that are applied under the oil well are processed with screw thread; Bevel for welding is processed at the novel dual metal composite pipes two ends that surface gathering and transferring is used.
Beneficial effect of the present invention: novel dual metal composite pipes inner liner compound pipe outer wall pipe is a base material with the carbon steel or low alloy steel pipe, gives full play to good mechanical mechanics property of carbon steel tube or low alloy steel and inexpensive feature; With the anti-corrosive alloy material is inside liner, gives full play to the corrosion resisting property of corrosion resisting alloy excellence, thereby makes it have excellent corrosion resistance and good mechanical mechanics property.Novel dual metal composite pipes structure of the present invention and manufacture method thereof, the threaded collar joint that thoroughly solves when having the composite bimetal pipe use now connects sealing problem and composite bimetal pipe ground Welding Problems, enlarge the use field of composite bimetal pipe, save the cost of oil field development.
The composite bimetal pipe that adopts this scheme to make, the end is good stainless steel of corrosion resisting property or nickel-base material, can adopt with the same threaded collar joint of pure corrosion resistant alloy pipe to be connected or welding technique, can effectively, thoroughly solve the connectivity problem of the on-the-spot use of composite pipe.
Carry out then comparing with the pipe nipple welding manner with the intact composite pipe of general making, this scheme is carried out the welding of outer wall pipe and pipe nipple earlier, only relates to the welding of two kinds of materials, pipe and pipe nipple weld seam in the welding of back, be end face seal structure, welded structure is simple, is again the welding of same material.The weld seam of outer wall pipe 1 and internal lining pipe 2 can adopt extraordinary welding methods such as friction welding or instantaneous liquid-phase diffusion welding, and parameter is controlled easily, the easy automation of process, and joint performance is good.Welding quality guarantees easily.
The scheme of this invention is also carried out the hydrostatic test to pipe, and three effects are arranged: the one, can test the bearing capacity of composite bimetal pipe; The 2nd, utilize gap and residual gas between hydraulic test pressure elimination outer wall pipe 1 and the internal lining pipe 2, it is tightr that inner and outer pipes is fitted; The 3rd, utilize the aperture on the outer tube, can check the leakage situation of inner wall tube.
This invention composite bimetal pipe makes the screw thread of field by using or is welded to connect the connection that becomes same material, and is simple in structure, and the quality of product height is realized interchangeable manufacturing, automation and batch process easily.It is easy to be used for the on-the-spot attended operation in oil field, the reliability height.
Below in conjunction with the drawings and specific embodiments the present invention is described in further detail.
Description of drawings
Fig. 1 is the structural profile schematic representation of novel dual metal composite pipes one end of the present invention, and the other end structure is identical.It is embodiment 1 structural representation.
Among the figure, 1. outer wall pipe, 2. internal lining pipe, 3. weld seam, 4. pipe nipple, 5. seal weld, 6. through hole.
Embodiment
Embodiment 1: consult accompanying drawing 1.The material of outer wall pipe 1 is a 16Mn low alloy steel, and outer wall pipe 1 internal diameter is 152.3 millimeters, and thickness is 8 millimeters, and length is 12000 millimeters.Internal lining pipe 2 materials are the 316L stainless steel, and internal lining pipe 2 external diameters are 150 millimeters, and thickness is 3 millimeters, and length is 12060 millimeters.Pipe nipple 4 is the stainless steel of 316L corrosion resistant material, and pipe nipple 4 internal diameters are 152.3 millimeters, and thickness is 11 millimeters, and length is 80 millimeters.
Be with internal lining pipe 2 in the outer wall pipe 1.The two ends of outer wall pipe 1 are welded with pipe nipple 4, between outer wall pipe 1 and the pipe nipple 4 weld seam 3 are arranged, and the two end part of internal lining pipe 2 are welded on the inwall of pipe nipple 4.On outer wall pipe 1 wall, be drilled with 3 diameters at 5 millimeters through hole 6.The described through hole 6 that bores on outer wall pipe 1 wall is course of working holes, adopts electric welding to weld dead through hole 6 after the hydrostatic test, and the novel dual metal composite pipes two ends are processed with screw thread or bevel for welding is processed at two ends.
The manufacture method of novel dual metal composite pipes:
1., outer wall pipe 1, pipe nipple 4 and internal lining pipe 2 processing and fabricatings: processing outer wall pipe 1 endoporus and pipe nipple 4 endoporus; The external diameter difference of outer wall pipe 1 endoporus, pipe nipple 4 endoporus and internal lining pipe 2 is 2.3 millimeters.
2., clean the outer surface of outer wall pipe 1 endoporus and internal lining pipe 2, remove degreasing and oxide;
3., adopt friction welding method to carry out welding between outer wall pipe 1 and the pipe nipple 4, remove reinforcement or burrs inside and outside the weld seam 3, butt welded seam 3 is heat-treated.
4., internal lining pipe 2 inserts in the outer wall pipe 1 and pipe nipple 4 that welds, and carries out compound;
5., the two ends with internal lining pipe 2 are welded on the inwall of pipe nipple 4 the two ends welding of pipe nipple 4 inwalls and internal lining pipe 2, formation seal angle weld seam;
6., seal, carry out the hydrostatic test, the pressure of the hydrostatic test is 29MPa at pipe nipple 4 two ends.
7., the novel dual metal composite pipes two ends are processed, be processed with screw thread, be used for the down-hole as the novel dual metal composite pipes two ends; If bevel for welding is processed at two ends, this novel dual metal composite pipes is used for ground transmission pipeline network construction.

Claims (3)

1, a kind of novel dual metal composite pipes, comprise outer wall pipe (1) and internal lining pipe (2), it is characterized in that internal lining pipe (2) is arranged in the outer wall pipe (1), the two ends of outer wall pipe (1) are welded with pipe nipple (4), between outer wall pipe (1) and the pipe nipple (4) weld seam (3) is arranged, the two end part of internal lining pipe (2) are welded on the inwall of pipe nipple (4), on outer wall pipe (1) wall, be drilled with the through hole (6) of at least 1 diameter at the 2-10 millimeter, the described through hole (6) that bores on outer wall pipe (1) wall is the course of working hole, adopt electric welding to weld dead through hole (6) after the hydrostatic test, be with electric welding through hole (6) to be mended in fact after the hydrostatic test, the novel dual metal composite pipes two ends are processed with screw thread or bevel for welding is processed at two ends.
2, novel dual metal composite pipes according to claim 1, it is characterized in that: the material of outer wall pipe (1) is a carbon steel or low alloy steel, the internal diameter of outer wall pipe (1) is between the 60-500 millimeter, the thickness of outer wall pipe (1) is between the 6-20 millimeter, internal lining pipe (2) material is stainless steel, nickel-base alloy or other corrosion resistant material, internal lining pipe (2) thickness is between 1 one 4 millimeters, pipe nipple (4) is a corrosion resistant material, and to have sufficiently high intensity and good weldability, as stainless steel, abros.
3, the manufacture method of novel dual metal composite pipes according to claim 1 is characterized in that:
1., outer wall pipe (1), pipe nipple (4) and internal lining pipe (2) processing and fabricating: outer wall pipe (1) endoporus is identical with pipe nipple (4) endoporus, and the external diameter difference of outer wall pipe (1) endoporus, pipe nipple (4) endoporus and internal lining pipe (2) is between the 1-3 millimeter;
2., clean the outer surface of outer wall pipe (1) endoporus and internal lining pipe (2), remove degreasing and oxide;
3., adopt welding methods such as melting, friction welding or instantaneous liquid-phase diffusion welding to carry out weld seam (3) between outer wall pipe (1) and the pipe nipple (4), remove reinforcement or burr inside and outside the weld seam (3), butt welded seam (3) is heat-treated in case of necessity;
4., internal lining pipe (2) inserts in the outer wall pipe (1) and pipe nipple (4) weld, carries out compound;
5., the two ends with internal lining pipe (2) are welded on the inwall of pipe nipple (4) the two ends welding of pipe nipple (4) inwall and internal lining pipe (2), formation seal angle weld seam;
6., pipe nipple (4) is sealed at both ends, carries out the hydrostatic test, the pressure of the hydrostatic test is between 5-30MPa;
7., the novel dual metal composite pipes two ends are processed, be processed with screw thread as the novel dual metal composite pipes two ends or bevel for welding is processed at two ends.
CNB200710118131XA 2007-06-29 2007-06-29 Novel dual metal composite pipes and manufacture method CN100549486C (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CNB200710118131XA CN100549486C (en) 2007-06-29 2007-06-29 Novel dual metal composite pipes and manufacture method

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CNB200710118131XA CN100549486C (en) 2007-06-29 2007-06-29 Novel dual metal composite pipes and manufacture method

Publications (2)

Publication Number Publication Date
CN101334119A true CN101334119A (en) 2008-12-31
CN100549486C CN100549486C (en) 2009-10-14

Family

ID=40196897

Family Applications (1)

Application Number Title Priority Date Filing Date
CNB200710118131XA CN100549486C (en) 2007-06-29 2007-06-29 Novel dual metal composite pipes and manufacture method

Country Status (1)

Country Link
CN (1) CN100549486C (en)

Cited By (13)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101915064A (en) * 2010-09-14 2010-12-15 衡阳华菱钢管有限公司 Bimetal compound pipe
CN102172803A (en) * 2011-03-25 2011-09-07 瑞安市乐勤航空部件有限公司 Magnesium alloy pipe and method for increasing intensity around weldment bead of magnesium alloy pipe
CN101876383B (en) * 2009-04-29 2012-12-12 北京安科管道工程科技有限公司 Composite metal pipe and manufacturing method thereof as well as composite pipeline formed therefrom
CN104384859A (en) * 2014-12-05 2015-03-04 邯郸新兴特种管材有限公司 Production method for nickel base alloy N06625 composite seamless steel pipe
CN104455760A (en) * 2014-09-23 2015-03-25 吴汉超 Manufacturing method for misplaced double-welding-layer double-metal compound pipe with stainless steel pipe joint
CN104976438A (en) * 2014-04-11 2015-10-14 北京安科管道工程科技有限公司 Outer end pipe used for composite metal pipe and manufacturing method of outer end pipe
CN105081541A (en) * 2015-09-11 2015-11-25 西安向阳航天材料股份有限公司 Method for producing semi-metallurgical metal composite tube through electric resistance welding
CN105276336A (en) * 2014-12-08 2016-01-27 中国石油天然气股份有限公司 Welding pipeline internal corrosion prevention method and pipeline used for method
CN105485438A (en) * 2016-02-18 2016-04-13 常熟市良益金属材料有限公司 High-nickel alloy pipe
CN107042246A (en) * 2016-04-28 2017-08-15 西北大学 A kind of method that utilization drawing method produces composite bimetal pipe
CN108591626A (en) * 2018-04-02 2018-09-28 苏州柏仕非奥自动化设备科技有限公司 A kind of processing and forming technology of carbon steel, Ni-based composite bimetal pipe part
CN108817854A (en) * 2018-05-24 2018-11-16 上海天阳钢管有限公司 A kind of process manufacturing compound oil well pipe hoop
CN110116296A (en) * 2019-03-28 2019-08-13 任耀文 A kind of production method of high temperature alloy thin-walled cooling cone component

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN201779363U (en) * 2010-09-14 2011-03-30 衡阳华菱钢管有限公司 Bi-metal composite delivery pipe

Cited By (15)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101876383B (en) * 2009-04-29 2012-12-12 北京安科管道工程科技有限公司 Composite metal pipe and manufacturing method thereof as well as composite pipeline formed therefrom
CN101915064A (en) * 2010-09-14 2010-12-15 衡阳华菱钢管有限公司 Bimetal compound pipe
CN102172803A (en) * 2011-03-25 2011-09-07 瑞安市乐勤航空部件有限公司 Magnesium alloy pipe and method for increasing intensity around weldment bead of magnesium alloy pipe
CN104976438A (en) * 2014-04-11 2015-10-14 北京安科管道工程科技有限公司 Outer end pipe used for composite metal pipe and manufacturing method of outer end pipe
CN104976438B (en) * 2014-04-11 2017-10-24 北京安科管道工程科技有限公司 Outer end pipe and its manufacture method for composite metal pipe
CN104455760A (en) * 2014-09-23 2015-03-25 吴汉超 Manufacturing method for misplaced double-welding-layer double-metal compound pipe with stainless steel pipe joint
CN104384859A (en) * 2014-12-05 2015-03-04 邯郸新兴特种管材有限公司 Production method for nickel base alloy N06625 composite seamless steel pipe
CN105276336A (en) * 2014-12-08 2016-01-27 中国石油天然气股份有限公司 Welding pipeline internal corrosion prevention method and pipeline used for method
CN105081541B (en) * 2015-09-11 2017-09-12 西安向阳航天材料股份有限公司 A kind of method that use electric resistance welding produces half metallurgy type metal composite pipe
CN105081541A (en) * 2015-09-11 2015-11-25 西安向阳航天材料股份有限公司 Method for producing semi-metallurgical metal composite tube through electric resistance welding
CN105485438A (en) * 2016-02-18 2016-04-13 常熟市良益金属材料有限公司 High-nickel alloy pipe
CN107042246A (en) * 2016-04-28 2017-08-15 西北大学 A kind of method that utilization drawing method produces composite bimetal pipe
CN108591626A (en) * 2018-04-02 2018-09-28 苏州柏仕非奥自动化设备科技有限公司 A kind of processing and forming technology of carbon steel, Ni-based composite bimetal pipe part
CN108817854A (en) * 2018-05-24 2018-11-16 上海天阳钢管有限公司 A kind of process manufacturing compound oil well pipe hoop
CN110116296A (en) * 2019-03-28 2019-08-13 任耀文 A kind of production method of high temperature alloy thin-walled cooling cone component

Also Published As

Publication number Publication date
CN100549486C (en) 2009-10-14

Similar Documents

Publication Publication Date Title
US4537429A (en) Tubular connection with cylindrical and tapered stepped threads
CA2685398C (en) Threaded joint with pressurizable seal
US7464449B2 (en) Method of forming a high-strength sealed connection for expandable tubulars
US5862866A (en) Double walled insulated tubing and method of installing same
US6042153A (en) Threaded connection for internally clad pipe
US6543816B1 (en) Threaded tubular joint proof to external pressure
US7014223B2 (en) Screw threaded joint for continuous-profile tubes
EP2609279B1 (en) Tubular threaded connection
CN100334383C (en) Coupling assembly and method
CN1189259C (en) Manufacture of bimetallic composite pipe
EP2486317B1 (en) A tubular joint having wedge threads with surface coating
US4705307A (en) Tubular goods joint
EP1106778A1 (en) Seal for expandable tubular connections
US4085951A (en) Hydril-type connector
CN101849079B (en) Threaded connection comprising at least one threaded element with an end lip for a metal tube
US6578880B2 (en) Wedgethread pipe connection
CN102071879B (en) Novel prestressed heat-insulation oil pipe
US20030067169A1 (en) Thread form with multifacited flanks
US20090226243A1 (en) Articulating joint with injector port
US4591195A (en) Pipe joint
US7793992B2 (en) Junction part for coaxial pipe elements, and a method of joining together coaxial pipe elements
EA015427B1 (en) Threaded joint for steel pipes
CN204677934U (en) A kind of novel alloy flange
CA2675894C (en) Threaded pipe connection
CN204187150U (en) Socket joint jointing type plastic lining steel-plastic composite pipe

Legal Events

Date Code Title Description
PB01 Publication
C06 Publication
SE01 Entry into force of request for substantive examination
C10 Entry into substantive examination
GR01 Patent grant
C14 Grant of patent or utility model