Prior art keywords
glass
panel
pillars
sheets
solder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
AU34444/93A
Other versions
AU3444493A (en
Inventor
Richard Edward Collins
Jian Zheng Tang
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SYDNEY THE, University of
Original Assignee
University of Sydney
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Sydney filed Critical University of Sydney
Priority to AU34444/93A priority Critical patent/AU659532B2/en
Priority claimed from PCT/AU1993/000040 external-priority patent/WO1993015296A1/en
Publication of AU3444493A publication Critical patent/AU3444493A/en
Application granted granted Critical
Publication of AU659532B2 publication Critical patent/AU659532B2/en
Anticipated expiration legal-status Critical
Expired legal-status Critical Current

Links

Classifications

    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02ATECHNOLOGIES FOR ADAPTATION TO CLIMATE CHANGE
    • Y02A30/00Adapting or protecting infrastructure or their operation
    • Y02A30/24Structural elements or technologies for improving thermal insulation
    • Y02A30/249Glazing, e.g. vacuum glazing
    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02BCLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO BUILDINGS, e.g. HOUSING, HOUSE APPLIANCES OR RELATED END-USER APPLICATIONS
    • Y02B80/00Architectural or constructional elements improving the thermal performance of buildings
    • Y02B80/22Glazing, e.g. vaccum glazing

Landscapes

  • Joining Of Glass To Other Materials (AREA)
  • Laminated Bodies (AREA)

Description

OPI DATE 01/09/93 AOJP DATE 28/10/93 APPLN. ID 34444/93 PCT NUMBER PCT/AU93/00040 AU9334444 JATY (PCT) (51) International Patent Classification 5 E06B 3/66 (11) International Publication Number: A (43) International Publication Date: WO 93/15296 5 August 1993 (05.08.93) (21) International Application (22) International Filing Date Number: PCT/AU93/00040 29 January 1993 (29.01.93) 31 January 1992 (31.01.92) AU Priority data: PL 0720 (71) Applicant (for all designated States except US): THE UNI- VERSITY OF SYDNEY [AU/AU]; Parramatta Road, Sydney, NSW 2006 (AU).
(72) Inventors; and Inventors/Applicants (for US only) COLLINS, Richard, Edward [AU/AU]; Cudgegong Road, Riverstone, NSW 2765 TANG, Jian, Zheng [CN/AU]; 8/3-7 Jubilee Avenue, Carlton, NSW 2218 (AU).
(74) Agent: GRIFFITH HACK CO.; G.P.O. Box 4164, Sydney, NSW 2001 (AU).
(81) Designated States: AT, AU, BB, BG, BR, CA, CH, DE, DK, ES, FI, GB, HU, JP, KP, KR, LK, LU, MG, MN, MW, NL, NO, PL, RO, RU, SD, SE, UA, US, European patent (AT, BE, CH, DE, DK, ES, FR, GB, GR, IE, IT, LU, MC, NL, PT, SE), OAPI patent (BF, BJ, CF, CG, CI, CM, GA, GN, ML, MR, SN, TD, TG), Published With international search report.
65953.
(54) Title: IMPROVEMENTS TO THERMALLY INSULATING GLASS PANELS 1 4\ ,o o o o 0 0 0 0 0 0 0 0 0 0 0 0 S 0 0 0 0 (57) Abstract This invention concerns a thermally insulating glass panel comprising two spaced apart sheets of glass 3) enclosing a low pressure space, and interconnected by a peripheral joint of fused solder glass and an array of pillars The pillars may be made entirely of metal. Alternatively the array may be made up of a combination of solder glass containing pillars and non-solder glass containing pillars. Additional support pieces may be arranged between the glass sheets 3) before the peripheral joint of solder glass is fused. A method of constructing such panels is also disclosed, as well as other variants.
WO 93/15296 PCr/AU93/0040 1 "IMPROVEMENTS TO THERMALLY INSULATIIG GLASS PANELS" TECHNICAL FIELD This invention concerns improvements to thermally insulating evacuated glass panels; these panels may be used for windows.
BACKGROUND ART Thermally insulating glass panels 1 typically comprise two spaced apart sheets of glass, 2 and 3, enclosing a low pressure space; refer to figures 1, 2 and 3 (not shown to scale). These sheets are interconnected by a peripheral joint of fused solder glass 4 and an array of pillars The pillars 5 ensure sufficient structural strength to withstand the forces imposed by atmospheric pressure, and maintain the sheets of glass spaced-apart. The pillars 5 comprise a preform 6 made of glass, ceramic, metal or other materia. s completely coated with a layer of solder glass 7. The preform 6 is usually made from the same material as the glass sheets in order that the thermal expansion coefficients of the preforms, the sheets and the solder glass should match. The purpose of the preform is to maintain the separation of the glass sheets during the fusion operation when the solder glass has little mechanical strength.
A pump-out tube 8 is incorporated into the panel and is used during the construction of the panel to evacuate the space between the glass sheets. The pump-out tube 8 is hermetically sealed by fused solder glass 9 to a hole which passes from an interior face of glass sheet 2 to the bottom of a recess 11 in the exterior face of glass sheet 2. The recess 11 allows the pump-out tube 8 to be melted and sealed leaving a stub which does not protrude WO 93/15296 PCT/AU93/00040 -2beyond the plane of the exterior face of the glass sheet 2.
A chemical getter 12 is often included within a machined recess 13 in one of the sheets of glass in the panel to counteract any rise in pressure due to outgassing from the glass.
A low emittance coating may be provided on the interior surface of one or both sheets of glass. The emittance of the coatings is usually between 0.05 to 0.2 to ensure a thermal conductance due to radiation of approximately 0.15 to 0.6 Wm' 2
K"
1 or less.
The internal pressure of the panel is usually below 10-2 torr and sometimes below 10-3 torr.
PILLAR DESIGN The design of the pillar array is a trade-off between reducing heat flow through the pillars (which imposes a requirement to reduce the number and size of the pillars) and reducing stresses within the panel and pillars (which requires more, and larger pillars).
A first sight, it would appear that the use of metal pillars would result in large heat transfer rates through the panel. Indeed, the thermal conductance of metal pillars is very large, due to the high thermal conductivity of the metal.
In the published literature, it is shown that a short circular contact between two bodies gives rise to a finite thermal impedance, equal to 2 Ka, where K is the thermal conductivity of the bodies and a is the radius of the contact. The existence of this finite thermal impedance arises because of the "spreading resistance" for heat flow within the bodies themselves. The thermal conductance values which apply to glass pillars of zero height also apply to metal pillars, and it has surprisingly been found that the actual heat flow through WCP 93/15296 PCT/AU93/00040 a metal pillar is quite low; it is almost exactly equal to the thermal conductance of a glass pillar of zero height.
It has therefore been realised that it is possible to design a pillar array using metal pillars, which has adequately low thermal conductance, for which external mechanical stresses are low, and for which internal fracture near the pillars is unlikely to occur.
Accordingly, a first aspect of the present invention, as currently envisaged, provides a thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint of fused solder glass and an array of pillars, wherein at least some of the pillars are made entirely of metal.
Preferably the diameter of the metal pillars is 0.2 millimetres or less, for instance 0.1 millimetres. The stress within the panel is affected by the glass thickness, and for 4mm thick glass sheets the pillar spacing is preferably between 15 and 30 millimetres. A smaller range of between 19 and 23 millimetres is also advantageous. Of course for different glass thicknesses different ranges are possible. The size of pillars and spacing of the array will give a heat flow of less than 0.3 Wm 2
K
1 and ensure sufficient structural strength to withstand the forces imposed by atmospheric pressure.
Preferably some, limited, inelastic deformation of the metal pillars occurs during construction of the panel. This will accommodate planar irregularities between the two glass sheets ensuring good physical contact between the pillars and the glass sheets.
Preferably the metal pillars are nickel, iron, molybdenum, tungsten, tantalum, titanium, aluminium, steel or stainless alloys containing these metals. These WO 93/15296 PCr/AU93/00040 4 metals ensure thermal performance and structural strength for the preferred pillar sizing and array geometry.
An embodiment of this aspect of the invention will now be described with reference to figures 4, 5 and 6.
Panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by an array of pillars Values of pillar separation and pillar radius, which achieve low external stresses, low probability of internal fracture near the pillars, and a heat flow for the entire pillar array less than 0.3 Wmf2K are shown in Figure 6. Typical values for the dimensions of an array of metal pillars are: Pillar separation 23 mm Pillar diameter 0.2 mm There is considerable flexibility in the choice of materials for the metal pillars disclosed here. The pillars must be strong enough to resist the compressive forces due to atmospheric forces. It is noted, however, that some limited inelastic deformation of the pillars when the vacuum is initially applied is tolerable and, indeed, may be advantageous. Such deformation compensates for minor variations in planarity of the glass sheets, and results in good mechanical contact between the pillar and the glass, thus evenly distributing the load over the pillar surface.
The material of the pillars should be compatible with the high temperature processing of the window (-500 0 C for 1 hour) and must have a low vapour pressure in order not to degrade the vacuum.
Suitable metals which satisfy these design constraints include: nickel, iron, molybdenum, tungsten, tantalum, titanium, aluminium and alloys containing these materials, such as steel, and stainless steel.
WIO 93/15296 P~r/U93/00040 5 CONTROL OF SEPARATION OF-GLASS SHEETS The separation of the glass sheets must be maintained when the solder glass is fused.
Hybrid Pillar Array According to another aspect of the present invention, as currently envisaged, there is provided a thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint of fused solder glass and an array of pillars; wherein the array of pillars is made up of a combination of solder glass containing pillars and non-solder glass containing pillars.
Advantageously the solder glass containing pillars have an expansion coefficient matched to the sheets of glass.
Preferably the non-solder glass containing pillars contain glass, ceramic or metal materials. The non-solder glass containing pillars maintain the spacing between the two glass sheets when the solder glass is melted.
An embodiment of this aspect of the invention will now be described with reference to figures 7 and 8.
Panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by an array of pillars. Some pillars 16 contain solder glass, but a small proportion of pillars 17 do not contain solder glass, and do not melt when the solder glass is fused.
The non-solder glass containing pillars 17 maintain the separation between the glass sheets during solder glass fusion. All the pillars 16 and 17 maintain the separation between the glass sheets after solder glass fusion when the panel has been evacuated and is w6 93/15296 PC/AU9/00040 93659 subject to atmospheric pressures.
Metal is a preferred material for the non-solder glass containing pillars. However, metal pillars exhibit larger heat flow than solder glass pillars of comparable diameter, but the increase in total heat flow through the array is relatively small if the fraction of metal pillars is not large.
Solder Glass Pillar Array As an alternative, according to this aspect of the present invention, as currently envisaged, there is provided a thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint of fused solder glass and an array of solder glass containing pillars; wherein support pieces are arranged between the glass sheets before the peripheral joint of solder glass is fused to maintain the spacing between the two glass sheets during solder glass fusion.
Preferably the support pieces break up when the low pressure space is subsequently created after the solder glass fusion. The break up of the support pieces prevents subsequent heat conduction through them, leading to an overall better thermal performance of the glass panel.
The support pieces may be made of glass, ceramic or metal materials.
An embodiment of this aspect of the invention will now be described with reference tc figures 9 and Referring now to figures 9 and 10, panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by an array of solder glass containing pillars 18. In addition support pieces 19 are used during the fabrication of the panel 1.
WO 93/15296 PC/AU9300040 -7- The support pieces 19 are made from glass, ceramic or metal materials. They may have one or more of several geometric forms, including spheres, rods, or hollow tubes.
The supports must be sufficiently strong to support the glass sheets when the solder glass is in its melted state. However, they do not need to be strong enough to support the load du*e to the vacuum as this may be totally borne by the norial support pillars. In the case the supports break when the vacuum is applied. The pieces will then fall to the bottom of the panel and play no further part.
A METHOD OF CONSTRUCTING A THERMALLY INSULATING GLASS PANEL Also according to this aspect of the present invention, as currently envisaged, there is provided a method of constructing a thermally insulating glass panel comprising two spaced apart sheets of glass enclosing a low pressure space interconnected by a peripheral joint of fused solder glass and an array of pillars, the method including the steps of: depositing a strip of solder glass around the periphery of the sheets; depositing an array of pillars onto one of the sheets tif glass; arranging support pieces between the sheets of glass; then bringing the glass sheets together, or permitting them to move together until the sheets come into contact with the support pieces; heating the panel to melt the solder glass; and creating a low pressure space between the WO93/15296 PCr/AU93/00040 8 glass sheets.
The support pieces maintain the spacing between the two glass sheets when solder glass is fused, but may break up under the load of forces resulting from atmospheric pressure when the low pressure space is created.
REDUCTION OF STRESS IN THE PANEL The mechanical stresses in evacuated panels are quite complex, and arise from several different sources.
Atmospheric pressure produces large stresses in the support pillars, and in the glass sheets immediately adjacent to the pillars. The nature of these stresses is well understood in the context of Hertzian indenter fracture experiments. Atmospheric pressure also results in tensile stresses on the outside surfaces of the glass sheets, near the pillars.
The existence of temperature differences across the panel gives rise to significant bending stresses and shear stresses in the solder glass joint. Also, thermal short circuiting by the peripheral solder glass joint affects the stresses in the region of the edge.
Wind loading of the panel also produces external tensile stresses.
In the design of evacuated panels it is important to consider the resultant stress, since it is this which acts to cause fracture. It has been found that the mechanical stresses due to bending are greatest near the edges of the panel. This arises because of the complex way in which the tensile and compressive stresses in the glass sheets translate into shear stresses in the fused solder glass joint, and because the temperature differences across the glass sheets near the edges are different from those near the middle of the panel. All these factors cause stress in the panel to be more severe WO 93/15296 PCrAU93/00040 9near the edges, and the corners, than over the rest of the surface.
Three advantageous techniques for combating stress will now be explored: Pillar Density The density of pillars may be greater throughout some regions of the panel than others; in particular near the edges.
An embodiment will now be described with reference to figures 11 and 12.
Panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by an unevenly distributed array of pillars The pillar array is arrnged such that the density of pillars 20 near the peripheial fused solder glass joint of the panel 1 is greater than towards the centre of the panel 1. This provides additional structural support in the regions of the panel subject to greater resultant stress. The tensile stresses near the edge of the panel are reduced significantly by increasing the density of support pillars near the edge. This occurs because the level of tensile stress above each support pillar in the edge region is reduced, with a consequent reduction in the total tensile stress.
Reductions in stresses near the edges can also be achieved by incorporating into the duvice, near the edges, pillars which are less compliant than the majority of the pillars in the array. Less compliant pillars can be of the same material as that of the rest of the array and of larger area, or of a different, less compliant material. The effect of including such pillars is to increase the area of the window over which bending deformation due to atmospheric pressure occurs, and to w6 93/15296i PPr/AU93/00040 10 decrease the magnitude of the tensile stresses associated with such deformation.
It is recognised, of course, that increased heat transfer occurs because of the greater number, or larger size, of support pillars. However, the increase is relatively small in terms of the overall insulating performance of the structure, and is more than outweighed by the beneficial effects from the reduced stresses.
Pre-Stressing The panel may be prestressed before the solder glass is fused. For instance compressive stress built into tie panel reduces the effect of external tensile stress.
An embodiment will now be described with reference to figures 13 and 14.
Panel 1 comprises two spaced apart glass sheets 21 and 22. The sheets are interconne-ted by a peripheral joint 4 of fused solder glass, and by array of pillars Tensile stress can be reduced by establishing compressive stress, during manufacture, in thac region of the panel when tensile stress will subsequently occur.
For example, if the glass sheet 21 will ultimately be installed on the outside of a building in a cold climate, the panel is bent throughout the fusion operation to provide a concave shape on the exterior surface of sheet 21. The magnitude of the pretensioning should not be such as to cause serious stresses in the panel. For example, for stresses less than 4 MPa, the probability of failure of the panel is negligible. When a prestressed window is installed, the compressive stress on the ovtside serves as an offset which increases the ability of the device to withstand temperature differences whilst maintaining external stresses below specified levels.
WO 93/15296 PCr/AU93/00040 11 Stiffening the Edges The edge regions of at least one sheet of glass may bE. thickened. The thickness of the sheets of glass may be increased around the edges of the glass panel by fixing, with adhesive, a plate to one or both sides of the edge region of at least one of the glass sheets.
The bending stiffness of a beam is a function of its thickness, varying inversely with the cube of the thickness. A relatively small increase in the thickness of the edges of the panel therefore results in significant stiffening of the structure as a whole. This stiffening can be used to reduce the overall bending of the device to the point where the external stresses on the hot side are very small. In addition, the existence of the bonded edge significantly reduces the tensile stresses in the glass sheets near the edge.
An embodiment will now be described with reference to figures 15 and 16.
Panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by array of pillars 23.
The thickness of the edge of the panel 1 is increased by bonding plates 24, with adhesive, to the external faces of both glass sheets. This reduces tensile stresses in the glass sheets near the edge, and reduces the resultant shear stress in the peripheral fused glass joint 4.
PUMP- OUT TUBE The design of the pump-out tube imposes particular challenges. Ideally, the tube should be very small, and located entirely within the nominal geometric dimensions of the evacuated window structure. However, small glass tubes can be extremely fragile and it is very difficult W6 93/15296 PCr/AU93/00040 12 to seal mechanically to such tubes during evacuation without breaking them.
According to a further aspect of t present invention, as currently envisaged, there is provided a thermally insulating glass panel comprising two spaced apart sheets of glass enclosing a low pressure space interconnected by a peripheral joint of fused solder glass and an array of pillars, and a pump-out tube to provide communication between the interior and the exterior of the panel during the creation of the low pressure space; wherein the pump-out tube extends through a hole extending from the bottom of a recess in the exterior face of one sheet of glass to the interior face of that sheet of glass, and the tube is joined to that sheet of glass by a solder glass joint made between the outside surface of the pump-out tube and the interior face of that sheet of glass.
The solder glass seal between the pump-out tube and the polished internal surface of the sheet of glass, is more effective than a seal to an abraded surface such as in the bottom of the recess. This is because the abraded glass surface contains many microcracks which extend some distance into the body of the glass. The solder glass may not completely close all these microcracks and very slow leaks can occur due to lateral motion of gas through the poorly connected microcrack region. By fusing the solder glass onto the smooth interior surface of the glass plates, this problem does not arise.
In addition the solder glass forms a smooth surface on the vacuum side, and is easily evacuated.
It will be appreciated that if the fused seal between the solder glass and the glass sheet is made on the inside of the glass plate, then the end of the pump- WO) 93/15296; Pe=/AU93/00040 13 out tube and the solder glass seal protrudes into the gap of the evacuated window. Since this gap is normally very small, there is a danger that the protrusion will contact onto the surface of the other glass sheet. In order to avoid this, a second recess may be machined onto the interior face of the other glass sheet in registration with the hole, to permit the extension of the pump-out tube to remain out of contact.
Preferably there is a fused solder glass joint between the two glass sheets extending partly around the hole. This provides local structural reinforcement around the pump-out hole and the recess.
An embodiment of this aspect of the invention will now be described with reference to figures 17 and 18.
Panel 1 comprises two spaced apart glass sheets 2 and 3. The sheets are interconnected by a peripheral joint 4 of fused solder glass, and by array of pillars The pump-out tube 8 is positioned in a hole drilled from the bottom of a machined recess 26 in the exterior face of one sheet of glass 2 to the interior face of that sheet of glass 2. The pump-out tube 8 is joined to that sheet of glass by an hermetic solder glass joint 27 made between the outside surface of the pump-out tube 8 and the interior face of sheet 2. A machined recess 28 in glass sheet 3, in registration with the pump-out tube hole, 25 provides clearance between the pump-out tube 8 and glass sheet 3.
The hole for the pump-out tube and the recesses give rise to stress magnification. In particular, under temperature differentials, or due to the effects of atmospheric pressure, the tensile stresses that are inevitably present in the glass are larger in the immediate vicinity of these features. In order to reduce the effect of this stress concentration the solder glass WO 93/15296 PCrAU93/000)40 14 deposited on the periphery of the glass sheezs, which forms the fused solder glass joint 4, may be extended 29 to partly surround the pump-out tube 8 and the recess 28.
A small gap 30 is left in the solder glass seal to permit the evacuation to take place. After fusion, solder glass 29 provides structural support around the pump-out tube 8. The existence of this soldez glass around the pumpout tube results in almost complete elimination of mechanical tensile stresses due to bending or atmospheric pressure and has a highly advantageous effect in the reduction of the probability of failure due to stress magnification by the pump-out tube recess.
After the space in the interior of the panel has been evacuated, the part of the tube 8 inside recess 26 is heated until it melts and is then sealed (tipped-off).
It can be seen, in Figure 17, that the tube 8 when tipped off does not protrude beyond the surface of glass sheet 2. The reason for this is so that when the panel is framed tube 8 will not be damaged by the frame, and is protected by the frame. The stub of the pump-out tube may be encapsulated or otherwise protected prior to mounting in the frame, in order to facilitate handling without damage.
A variant of the technique for sealing the pumpout tube, is to polish the inside of the recess in which the end of the pump-out tube is located. The polished surface 31 of the recess is suitable for the solder glass sealing operation, being smooth. In this case, a satisfactory seal can be made on the exterior surface of the glass, as shown in figure 19.

Claims (22)

1. A thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint of fused solder glass and an array of pillars; wherein at least some of the pillars are made entirely of metal.
2. A panel according to claim 1 wherein for 4 millimetre thick glass sheets the pillar diameters range from 0.1 to 0.2 millimetres, and the pillar spacings range from 15 to 30 millimetres.
3. A panel according to claim 1 or 2, wherein some inelastic deformation of the metal pillars occurs during construction of the panel.
4. A panel according to any preceding claim, wherein the metal is nickel, iron, molybdenum, tungsten, tantalum, titan,um, aluminium, steel or a stainless alloy containing these metals.
5. A thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint of fused solder glass and an array of pillars; wherein the array of pillars is made up of a combination of solder glass containing pillars and non-solder glass containing pillars.
6. A panel according to claim 5, wherein the solder glass containing pillars contain glass, ceramic or metal materials.
7. A thermally insulating glass panel comprising: two spaced apart sheets of glass enclosing a low pressure space and interconnected by a peripheral joint WO 93/15296 WO093/15296 PCr/AU93/00040 16 of fused solder glass and an array of solder glass containing pillars; wherein support pieces are arranged between the glass sheets before the peripheral joint of solder glass is fused.
8. A panel according to claim 7, wherein the support pieces maintain the spacing between the glass sheets when the solder glass is fuse.J, but break up when the low pressure is subsequently created.
9. A pa:iel according to claim 8, wherein the support pieces are made from glass, ceramic, or metal materials.
A method of constructing a thermally insulating glass panel comprising two spaced apart sheets of glass enclosing a low pressure space interconnected by a peripheral joint of fused solder glass and an array of pillars, the method including the steps of: depositing a strip of solder glass around the periphery of the glass sheets; depositing an array of pillars onto one of the sheets of glass; arranging support pieces between the sheets of glass; then bringing the glass sheets together, or permitting them to move until the sheets come into contact with the support pieces; heating the panel to melt the solder glass; and creating a low pressure space between the glass sheets.
11. A method according to Claim 10, wherein the ,support pieces maintain the spacing between the two sheets of glass when the solder glass is fused but break up when the low pressure space is created. 17
12. A method according to Claim 10, wherein the support pieces are made from glass, ceramic or metal materials.
13. A panel according to any one of claims 1 to 9, wherein the density of pillars is greater throughout some regions of the panel than others.
14. A panel according to any one of claims 1 to 9, wherein the pillars are less compliant in some regions of the panel than others.
15. A panel according to any one of claims 1 to 9, wherein the panel is prestressed before the solder glass is fused.
16. A panel according to any one of claims 1 to 9, wherein edge regions of at least one glass sheet are thickened.
17. A panel according to claim 16, wherein a plate is fixed by adhesive to one or both sides of the edge region of at least one of the glass sheets to thicken it.
18. A thermally insulating glass panel, comprising: 20 two spaced apart sheets of glass enclosing a low *fle '..pressure space and interconnected by a peripheral joint of fused solder glass and an array of pillars, and a pump-out tube to provide communication between the interior and the exterior of the panel during the creation of the low pressure space; S. wherein the pump-out tube extends through a hole extending from the bottom of a recess in the exterior face of one sheet of glass to the interior face of that sheet of glass, and the tube is joined to that sheet of glass by a solder glass joint made between the outside surface of the pump-out tube and the interior face of that sheet of glass.
19. A panel according to claim 18, wherein a recess is provided on the interior face of the other sheet of glass in registration with the hole. A panel according to claim 18, wherein there is a fused solder glass joint between the two glass sheets, which extends partly around the hole.
S:04828XL 18
21. A thermally insulating glass panel substantially as herein described with reference to the accompanying drawings.
22. A method of constructing a thermally insulating glass panel substantially as herein described with reference to the accompanying drawings. DATED this 13th day of March 1995 THE UNIVERSITY OF SYDNEY By their Patent Attorneys GRIFFITH HACK CO. S:04828XL
AU34444/93A 1992-01-31 1993-01-29 Improvements to thermally insulating glass panels Expired AU659532B2 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
AU34444/93A AU659532B2 (en) 1992-01-31 1993-01-29 Improvements to thermally insulating glass panels

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
AUPL072092 1992-01-31
AUPL0720 1992-01-31
AU34444/93A AU659532B2 (en) 1992-01-31 1993-01-29 Improvements to thermally insulating glass panels
PCT/AU1993/000040 WO1993015296A1 (en) 1992-01-31 1993-01-29 Improvements to thermally insulating glass panels

Publications (2)

Publication Number Publication Date
AU3444493A AU3444493A (en) 1993-09-01
AU659532B2 true AU659532B2 (en) 1995-05-18

Family

ID=25622890

Family Applications (1)

Application Number Title Priority Date Filing Date
AU34444/93A Expired AU659532B2 (en) 1992-01-31 1993-01-29 Improvements to thermally insulating glass panels

Country Status (1)

Country Link
AU (1) AU659532B2 (en)

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1996012862A1 (en) * 1994-10-19 1996-05-02 The University Of Sydney Design improvements to vacuum glazing
AU673610B2 (en) * 1993-06-30 1996-11-14 University Of Sydney, The Methods of construction of evacuated glazing
EP1965013A2 (en) * 1999-06-10 2008-09-03 The University Of Sydney Glass panel

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU686461B2 (en) * 1994-10-19 1998-02-05 University Of Sydney, The Design improvements to vacuum glazing

Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU4055493A (en) * 1993-04-21 1994-11-08 Kenneth R. Parker Insulating panel

Patent Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU4055493A (en) * 1993-04-21 1994-11-08 Kenneth R. Parker Insulating panel

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU673610B2 (en) * 1993-06-30 1996-11-14 University Of Sydney, The Methods of construction of evacuated glazing
WO1996012862A1 (en) * 1994-10-19 1996-05-02 The University Of Sydney Design improvements to vacuum glazing
EP1965013A2 (en) * 1999-06-10 2008-09-03 The University Of Sydney Glass panel
EP1965013A3 (en) * 1999-06-10 2012-10-03 The University Of Sydney Glass panel

Also Published As

Publication number Publication date
AU3444493A (en) 1993-09-01

Similar Documents

Publication Publication Date Title
US5664395A (en) Thermally insulating glass panels
EP1506945B1 (en) Translucent glass panel
JP4251609B2 (en) Glass panel
AU673610B2 (en) Methods of construction of evacuated glazing
EP2099997B1 (en) Vacuum ig window unit with metal member in hermetic edge seal
EP1171397B1 (en) Method of sealing glass
US5027574A (en) Thermally insulating structure
US5657607A (en) Thermally insulating glass panel and method of construction
EP1508551B1 (en) Method of manufacturing glass panel, and glass panel manufactured by the method
US20090155499A1 (en) Metal-inclusive edge seal for vacuum insulating glass unit, and/or method of making the same
CA1290624C (en) Insulating glass unit
WO2001090525A1 (en) Vacuum ig window unit with spacers between first and second edge seals
AU2012292347B2 (en) Glazing unit with peripheral seal and corresponding manufacturing process
JP2005200301A (en) Improvement of vacuum-sealed double-glazed unit
WO1991002878A1 (en) A thermally insulating glass panel and method of construction
WO2001027430A1 (en) Vacuum ig window unit with dual peripheral seal
WO2013048981A1 (en) Vacuum insulating glass (vig) unit pump-out tube protecting techniques, and/or vig units incorporating the same
US20180305972A1 (en) Vacuum insulated glass unit with glass-to-metal seal and methods of assembling same
JP2005320229A (en) Pressure reduced glass lined panel and method of manufacturing the same
AU659532B2 (en) Improvements to thermally insulating glass panels
WO2000066868A1 (en) Vacuum insulating glazing spacer pillar with diamond-like carbon coating
JPWO2003000613A1 (en) Manufacturing method of glass panel
EP3786129A1 (en) Glass panel unit and glass window
WO2021059167A1 (en) Low thermal conductivity metal-polymer-metal sandwich composite spacer system for vacuum insulated glass (vig) units, vig units including composite spacers, and methods of making the same
EP3906351B1 (en) Sealant in a vacuum insulated glazing unit